| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | P(3) | Ni(4) | Al | S | Sb | Si | |
|
(1) In determining Cu min., Cu may be calculated as Cu + Ni. (2) Cu + Sum of Named Elements 99.0% min. (3) For continuous castings P shall be 1.5% max. (4) Ni value includes Co. |
|||||||||||
| Min (%) | 82.0 | 7.0 | 7.0 | ||||||||
| Max (%) | 85.0 | 9.0 | 9.0 | 0.8 | 0.20 | 0.50 | 1.0 | 0.005 | 0.08 | 0.50 | 0.005 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load | Izod (ft-lbs) |
Compressive Strength .1 in. set/in. (ksi) |
Fatigue Strength** (ksi) |
Proportional Limit (ksi) |
|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||
| As Continuous Cast | As Continuous Cast | M07 |
34 Min for Standard |
20 Min for Standard |
8 Min for Standard |
|||||
| As Sand Cast | As Sand Cast | M01 |
25 Min 32 Typ |
12 Min 16 Typ |
8 Min 20 Typ |
60 Typ |
5 Typ | 48 Typ | 15 Typ | 8 Typ |
| Densitylb/cu in. at 68°F | 0.32 |
|---|---|
| Specific Gravity | 8.86 |
| Electrical Conductivity% IACS at 68°F | 12 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 33.6 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 10 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 11000 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | High |
| Drossing | Low |
| Effect of Section Size | Medium |
| Fluidity | High |
| Gassing | Medium |
| Patternmakers Shrinkage inches per inch | 3/16 |
| Shrinkage in Solidification | Low |
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Machinability Rating | 70 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 500 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Fasteners | Washers | Corrosion Resistance | Corrosion Resistance |
| Washers | Friction & Wear Properties | Wear Resistance | |
| Washers | Mechanical Properties | Relatively Low Strength | |
| Industrial | Bearings | Bearing Properties | Bearing Wear Resistance |
| Bearings | Corrosion Resistance | Corrosion Resistance | |
| Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bearings | Friction & Wear Properties | Anti-Seizing Properties | |
| Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Bearings | Friction & Wear Properties | Wear Resistance | |
| Bearings | Mechanical Properties | Relatively Low Strength | |
| Bushings | Corrosion Resistance | Corrosion Resistance | |
| Bushings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bushings | Friction & Wear Properties | Anti-Seizing Properties | |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Bushings | Mechanical Properties | Relatively Low Strength | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Corrosion Resistant Castings | Friction & Wear Properties | Wear Resistance | |
| Corrosion Resistant Castings | Machining Properties | Machinability, Good | |
| Corrosion Resistant Castings | Mechanical Properties | Relatively Low Strength | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Pump Impellers | Friction & Wear Properties | Wear Resistance | |
| Pump Impellers | Machining Properties | Excellent Machinability | |
| Slide Bars | Corrosion Resistance | Corrosion Resistance | |
| Slide Bars | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Slide Bars | Friction & Wear Properties | Anti-Seizing Properties | |
| Slide Bars | Friction & Wear Properties | Wear Resistance | |
| Slide Bars | Mechanical Properties | Relatively Low Strength |
Applicable Specifications
Corrosion Properties