Find suppliers for this alloy
C93500
| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | P(3) | Ni(4) | Al | S | Sb | Si | |
|
(1) In determining Cu min., Cu may be calculated as Cu + Ni. (2) Cu + Sum of Named Elements 99.0% min. (3) For continuous castings P shall be 1.5% max. (4) Ni value includes Co. |
|||||||||||
| Min (%) | 83.0 | 8.0 | 4.3 | ||||||||
| Max (%) | 86.0 | 10.0 | 6.0 | 2.0 | 0.20 | 0.05 | 1.0 | 0.005 | 0.08 | 0.30 | 0.005 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load | Charpy V-Notch Impact Strength (ft-lbs) |
Compressive Strength .001 in. set/in. (ksi) |
|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||||
| As Centrifugal Cast | As Centrifugal Cast | M02 |
28 Min for Standard 28 Min for Standard |
12 Min for Standard |
15 Min for Standard 15 Min for Standard |
|||
| As Continuous Cast | As Continuous Cast | M07 |
30 Min for Standard 30 Min for Standard |
16 Min for Standard |
12 Min for Standard 12 Min for Standard |
|||
| As Sand Cast | As Sand Cast | M01 |
28 Min for Standard 28 Min for Standard 32 Typ |
12 Min for Standard 16 Typ |
15 Min for Standard 15 Min for Standard 20 Typ |
60 Typ |
8 Typ |
13 Typ |
| Melting Point - Liquidus°F | 1830 |
|---|---|
| Melting Point - Solidus°F | 1570 |
| Densitylb/cu in. at 68°F | 0.32 |
| Specific Gravity | 8.86 |
| Electrical Conductivity% IACS at 68°F | 15 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 40.7 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 9.9 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 14500 |
| Incipient Melting°F | 600 |
| Magnetic Permeability | 1 |
Casting Characteristics
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Machinability Rating | 70 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 500 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Automotive | Backing for Babbitt Lined Bearings | Corrosion Resistance | Corrosion Resistance |
| Backing for Babbitt Lined Bearings | Friction & Wear Properties | Wear Resistance | |
| Backing for Babbitt Lined Bearings | Mechanical Properties | Relatively Low Strength | |
| Industrial | Bearings | Corrosion Resistance | Corrosion Resistance |
| Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bearings | Friction & Wear Properties | Anti-Seizing Properties | |
| Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Bearings | Friction & Wear Properties | Wear Resistance | |
| Bearings | Machining Properties | Excellent Machinability | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Corrosion Resistant Castings | Friction & Wear Properties | Wear Resistance | |
| Corrosion Resistant Castings | Machining Properties | Excellent Machinability | |
| High Speed, Light Load Bushings | Corrosion Resistance | Corrosion Resistance | |
| High Speed, Light Load Bushings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| High Speed, Light Load Bushings | Friction & Wear Properties | Anti-Seizing Properties | |
| High Speed, Light Load Bushings | Friction & Wear Properties | Low Coefficient of Friction | |
| High Speed, Light Load Bushings | Friction & Wear Properties | Wear Resistance | |
| High Speed, Light Load Bushings | Machining Properties | Excellent Machinability | |
| Mild Acidic Applications | Corrosion Resistance | Corrosion Resistance | |
| Mild Acidic Applications | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Mild Acidic Applications | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Mild Acidic Applications | Friction & Wear Properties | Wear Resistance | |
| Mild Acidic Applications | Machining Properties | Excellent Machinability | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Pump Impellers | Friction & Wear Properties | Wear Resistance | |
| Pump Impellers | Machining Properties | Excellent Machinability |
Applicable Specifications
Corrosion Properties