Find suppliers for this alloy
C93600
| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P(2) | Ni(3) | Al | S | Sb | Si | |
|
(1) Cu + Sum of Named Elements 99.3% min. (2) For continuous castings P shall be 1.5% max. (3) Ni value includes Co. |
|||||||||||
| Min (%) | 79.0 | 11.0 | 6.0 | ||||||||
| Max (%) | 83.0 | 13.0 | 8.0 | 1.0 | 0.20 | 0.15 | 1.0 | 0.005 | 0.08 | 0.55 | 0.005 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| As Centrifugal Cast | As Centrifugal Cast | M02 |
32 Min for Standard 35 Typ |
16 Min for Standard 21 Typ |
10 Min for Standard 15 Typ |
65 Typ |
| As Continuous Cast | As Continuous Cast | M07 |
33 Min for Standard 35 Typ |
20 Min for Standard 21 Typ |
10 Min for Standard 15 Typ |
65 Typ |
| As Permanent Mold Cast | As Permanent Mold Cast | M05 |
35 Typ |
21 Typ |
15 Typ |
65 Typ |
| Melting Point - Liquidus°F | 1720 |
|---|---|
| Melting Point - Solidus°F | 1550 |
| Densitylb/cu in. at 68°F | 0.325 |
| Specific Gravity | 9 |
| Electrical Conductivity% IACS at 68°F | 11 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 28.5 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 10.3 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 14000 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | High |
| Drossing | Low |
| Effect of Section Size | Low |
| Fluidity | High |
| Gassing | Medium |
| Patternmakers Shrinkage inches per inch | 2/16 |
| Shrinkage in Solidification | Low |
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Machinability Rating | 80 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 500 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Backs for Lined Bearings | Corrosion Resistance | Corrosion Resistance |
| Backs for Lined Bearings | Friction & Wear Properties | Wear Resistance | |
| Backs for Lined Bearings | Machining Properties | Machinability, Good | |
| Bearings for corrosion, lubrication or pressure | Corrosion Resistance | Corrosion Resistance | |
| Bearings for corrosion, lubrication or pressure | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Bearings for corrosion, lubrication or pressure | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Bearings for corrosion, lubrication or pressure | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bearings for corrosion, lubrication or pressure | Friction & Wear Properties | Anti-Seizing Properties | |
| Bearings for corrosion, lubrication or pressure | Friction & Wear Properties | Low Coefficient of Friction | |
| Bearings for corrosion, lubrication or pressure | Friction & Wear Properties | Wear Resistance | |
| Bearings for corrosion, lubrication or pressure | Machining Properties | Excellent Machinability | |
| Bushings for corrosion, lubrication or pressure | Corrosion Resistance | Corrosion Resistance | |
| Bushings for corrosion, lubrication or pressure | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Bushings for corrosion, lubrication or pressure | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Bushings for corrosion, lubrication or pressure | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bushings for corrosion, lubrication or pressure | Friction & Wear Properties | Anti-Seizing Properties | |
| Bushings for corrosion, lubrication or pressure | Friction & Wear Properties | Low Coefficient of Friction | |
| Bushings for corrosion, lubrication or pressure | Friction & Wear Properties | Wear Resistance | |
| Bushings for corrosion, lubrication or pressure | Machining Properties | Excellent Machinability | |
| Cam Bushings for Diesel Engines | Corrosion Resistance | Corrosion Resistance | |
| Cam Bushings for Diesel Engines | Friction & Wear Properties | Wear Resistance | |
| Cam Bushings for Diesel Engines | Machining Properties | Machinability, Good | |
| Crankshaft Main Bearings | Corrosion Resistance | Corrosion Resistance | |
| Crankshaft Main Bearings | Friction & Wear Properties | Anti-Seizing Properties | |
| Crankshaft Main Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Crankshaft Main Bearings | Machining Properties | Machinability, Good | |
| Deep Well Pump Bowl Bushings | Corrosion Resistance | Corrosion Resistance | |
| Deep Well Pump Bowl Bushings | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Deep Well Pump Bowl Bushings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Deep Well Pump Bowl Bushings | Friction & Wear Properties | Wear Resistance | |
| Deep Well Pump Bowl Bushings | Machining Properties | Machinability, Good | |
| Deep Well Pump Line Shaft Bearings | Corrosion Resistance | Corrosion Resistance | |
| Deep Well Pump Line Shaft Bearings | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Deep Well Pump Line Shaft Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Deep Well Pump Line Shaft Bearings | Friction & Wear Properties | Wear Resistance | |
| Deep Well Pump Line Shaft Bearings | Machining Properties | Machinability, Good | |
| Electric Motor Bearings | Corrosion Resistance | Corrosion Resistance | |
| Electric Motor Bearings | Friction & Wear Properties | Anti-Seizing Properties | |
| Electric Motor Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Electric Motor Bearings | Friction & Wear Properties | Wear Resistance | |
| Electric Motor Bearings | Machining Properties | Machinability, Good | |
| Flow Monitor Valves | Corrosion Resistance | Corrosion Resistance | |
| Flow Monitor Valves | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Flow Monitor Valves | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Flow Monitor Valves | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Flow Monitor Valves | Friction & Wear Properties | Wear Resistance | |
| Flow Monitor Valves | Machining Properties | Excellent Machinability | |
| Guide Bushings for Piston Rods | Corrosion Resistance | Corrosion Resistance | |
| Guide Bushings for Piston Rods | Friction & Wear Properties | Anti-Seizing Properties | |
| Guide Bushings for Piston Rods | Friction & Wear Properties | Low Coefficient of Friction | |
| Guide Bushings for Piston Rods | Friction & Wear Properties | Wear Resistance | |
| Guide Bushings for Piston Rods | Machining Properties | Machinability, Good | |
| Guide Bushings for Valves | Corrosion Resistance | Corrosion Resistance | |
| Guide Bushings for Valves | Friction & Wear Properties | Anti-Seizing Properties | |
| Guide Bushings for Valves | Friction & Wear Properties | Low Coefficient of Friction | |
| Guide Bushings for Valves | Friction & Wear Properties | Wear Resistance | |
| Guide Bushings for Valves | Machining Properties | Machinability, Good | |
| Hydraulic Gland Seals | Corrosion Resistance | Corrosion Resistance | |
| Hydraulic Gland Seals | Friction & Wear Properties | Anti-Seizing Properties | |
| Hydraulic Gland Seals | Friction & Wear Properties | Low Coefficient of Friction | |
| Hydraulic Gland Seals | Friction & Wear Properties | Wear Resistance | |
| Hydraulic Gland Seals | Machining Properties | Machinability, Good | |
| Locomotive Bearing Parts | Corrosion Resistance | Corrosion Resistance | |
| Locomotive Bearing Parts | Friction & Wear Properties | Wear Resistance | |
| Locomotive Bearing Parts | Machining Properties | Machinability, Good | |
| Locomotive Bearing Parts | Mechanical Properties | Resistance to Pounding | |
| Main Bearings for Presses | Corrosion Resistance | Corrosion Resistance | |
| Main Bearings for Presses | Friction & Wear Properties | Anti-Seizing Properties | |
| Main Bearings for Presses | Friction & Wear Properties | Low Coefficient of Friction | |
| Main Bearings for Presses | Friction & Wear Properties | Wear Resistance | |
| Main Bearings for Presses | Machining Properties | Machinability, Good | |
| Oil Field Equipment | Corrosion Resistance | Corrosion Resistance | |
| Oil Field Equipment | Friction & Wear Properties | Anti-Seizing Properties | |
| Oil Field Equipment | Friction & Wear Properties | Tolerance for Dirt and Grit | |
| Oil Field Equipment | Friction & Wear Properties | Wear Resistance | |
| Oil Field Equipment | Machining Properties | Machinability, Good | |
| Piston Pin Bearings | Corrosion Resistance | Corrosion Resistance | |
| Piston Pin Bearings | Friction & Wear Properties | Anti-Seizing Properties | |
| Piston Pin Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Piston Pin Bearings | Friction & Wear Properties | Wear Resistance | |
| Piston Pin Bearings | Machining Properties | Machinability, Good | |
| Pump Sleeves | Corrosion Resistance | Corrosion Resistance | |
| Pump Sleeves | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Pump Sleeves | Friction & Wear Properties | Wear Resistance | |
| Rod Bushings | Corrosion Resistance | Corrosion Resistance | |
| Rod Bushings | Friction & Wear Properties | Anti-Seizing Properties | |
| Rod Bushings | Friction & Wear Properties | Low Coefficient of Friction | |
| Rod Bushings | Friction & Wear Properties | Wear Resistance | |
| Rod Bushings | Machining Properties | Machinability, Good | |
| Rolling Mill Bearings | Corrosion Resistance | Corrosion Resistance | |
| Rolling Mill Bearings | Friction & Wear Properties | Anti-Seizing Properties | |
| Rolling Mill Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Rolling Mill Bearings | Friction & Wear Properties | Wear Resistance | |
| Rolling Mill Bearings | Machining Properties | Machinability, Good | |
| Seals | Corrosion Resistance | Corrosion Resistance | |
| Seals | Friction & Wear Properties | Anti-Seizing Properties | |
| Seals | Friction & Wear Properties | Low Coefficient of Friction | |
| Seals | Friction & Wear Properties | Wear Resistance | |
| Seals | Machining Properties | Machinability, Good | |
| Sleeve Bushings (for cranes, etc.) | Corrosion Resistance | Corrosion Resistance | |
| Sleeve Bushings (for cranes, etc.) | Friction & Wear Properties | Anti-Seizing Properties | |
| Sleeve Bushings (for cranes, etc.) | Friction & Wear Properties | Low Coefficient of Friction | |
| Sleeve Bushings (for cranes, etc.) | Friction & Wear Properties | Wear Resistance | |
| Sleeve Bushings (for cranes, etc.) | Machining Properties | Machinability, Good | |
| Spacer Bushings (for Pumps, etc.) | Corrosion Resistance | Corrosion Resistance | |
| Spacer Bushings (for Pumps, etc.) | Friction & Wear Properties | Anti-Seizing Properties | |
| Spacer Bushings (for Pumps, etc.) | Friction & Wear Properties | Low Coefficient of Friction | |
| Spacer Bushings (for Pumps, etc.) | Friction & Wear Properties | Wear Resistance | |
| Spacer Bushings (for Pumps, etc.) | Machining Properties | Machinability, Good | |
| Steel Mill Bushings | Corrosion Resistance | Corrosion Resistance | |
| Steel Mill Bushings | Friction & Wear Properties | Anti-Seizing Properties | |
| Steel Mill Bushings | Friction & Wear Properties | Tolerance for Dirt and Grit | |
| Steel Mill Bushings | Friction & Wear Properties | Wear Resistance | |
| Steel Mill Bushings | Machining Properties | Machinability, Good | |
| Wrist Pin Bushings | Corrosion Resistance | Corrosion Resistance | |
| Wrist Pin Bushings | Friction & Wear Properties | Anti-Seizing Properties | |
| Wrist Pin Bushings | Friction & Wear Properties | Low Coefficient of Friction | |
| Wrist Pin Bushings | Friction & Wear Properties | Wear Resistance | |
| Wrist Pin Bushings | Machining Properties | Machinability, Good |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Centrifugal Cast | ASTM | B271/B271M | COPPER BASE ALLOY CENTRIFUGAL CASTINGS | ||
| As Continuous Cast | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | ||
| As Sand Cast | ASTM | B66 | BRONZE CASTINGS IN THE ROUGH FOR LOCOMOTIVE WEARING PARTS | ||
| MILITARY | MIL-C-22229 | COPPER BASE ALLOY CASTINGS (FOR PRESSURE TIGHT APPLICATIONS) | |||
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM |
Corrosion Properties