Find suppliers for this alloy
C93700
| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe(2) | P(3) | Ni(4) | Al | S | Sb | Si | |
|
(1) Cu + Sum of Named Elements 99.0% min. (2) Fe shall be 0.35% max. when used for steel-backed bearings (3) For continuous castings P shall be 1.5% max. (4) Ni value includes Co. |
|||||||||||
| Min (%) | 78.0 | 8.0 | 9.0 | ||||||||
| Max (%) | 82.0 | 11.0 | 11.0 | 0.8 | 0.7 | 0.10 | 0.50 | 0.005 | 0.08 | 0.50 | 0.005 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load | Shear Strength (ksi) |
Izod (ft-lbs) |
Charpy V-Notch Impact Strength (ft-lbs) |
Compressive Strength .001 in. set/in. (ksi) |
Compressive Strength .1 in. set/in. (ksi) |
Creep Strength (0.1% per 10,000 hours) (ksi) |
Fatigue Strength** (ksi) |
Proportional Limit (ksi) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | |||||||||||||||
| As Centrifugal Cast | As Centrifugal Cast | M02 |
30 Min for Standard 30 Min for Standard |
12 Min for Standard |
15 Min for Standard 15 Min for Standard |
||||||||||
| As Continuous Cast | As Continuous Cast | M07 |
35 Min for Standard 40 Min for Standard |
20 Min for Standard |
6 Min for Standard 6 Min for Standard |
||||||||||
| As Sand Cast | As Sand Cast | M01 |
30 Min for Standard 30 Min for Standard 35 Typ |
16 Typ |
12 Min for Standard 18 Typ |
15 Min for Standard 15 Min for Standard 20 Typ |
60 Typ |
18 Typ |
5 Typ | 11 Typ |
13 Typ | 47 Typ | 7.4 Typ | 13 Typ | 8 Typ |
| Melting Point - Liquidus°F | 1705 |
|---|---|
| Melting Point - Solidus°F | 1403 |
| Densitylb/cu in. at 68°F | 0.32 |
| Specific Gravity | 8.86 |
| Electrical Conductivity% IACS at 68°F | 10 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 27.1 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 10.3 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 11000 |
| Incipient Melting°F | 600 |
| Magnetic Permeability | 1 |
Casting Characteristics
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Machinability Rating | 80 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 500 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Builders Hardware | Brackets | Corrosion Resistance | Corrosion Resistance |
| Brackets | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Brackets | Machining Properties | Machinability, Good | |
| Brackets | Mechanical Properties | Relatively Low Strength | |
| Fasteners | Nuts | Corrosion Resistance | Corrosion Resistance |
| Nuts | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Nuts | Friction & Wear Properties | Wear Resistance | |
| Nuts | Machining Properties | Excellent Machinability | |
| Washers for Engines | Corrosion Resistance | Corrosion Resistance | |
| Washers for Engines | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Washers for Engines | Friction & Wear Properties | Wear Resistance | |
| Washers for Engines | Machining Properties | Excellent Machinability | |
| Industrial | Applications Requiring Acid Resistance to Sulphite Fluids | Corrosion Resistance | Corrosion Resistance |
| Applications Requiring Acid Resistance to Sulphite Fluids | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Applications Requiring Acid Resistance to Sulphite Fluids | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Applications Requiring Acid Resistance to Sulphite Fluids | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Applications Requiring Acid Resistance to Sulphite Fluids | Friction & Wear Properties | Wear Resistance | |
| Applications Requiring Acid Resistance to Sulphite Fluids | Machining Properties | Excellent Machinability | |
| Bearing Plates | Corrosion Resistance | Corrosion Resistance | |
| Bearing Plates | Friction & Wear Properties | Wear Resistance | |
| Bearing Plates | Machining Properties | Machinability, Good | |
| Bearing Plates | Mechanical Properties | Relatively Low Strength | |
| Bearings | Corrosion Resistance | Corrosion Resistance | |
| Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bearings | Friction & Wear Properties | Anti-Seizing Properties | |
| Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Bearings | Friction & Wear Properties | Wear Resistance | |
| Bearings | Machining Properties | Excellent Machinability | |
| Bushings | Corrosion Resistance | Corrosion Resistance | |
| Bushings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bushings | Friction & Wear Properties | Anti-Seizing Properties | |
| Bushings | Friction & Wear Properties | Low Coefficient of Friction | |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Bushings | Machining Properties | Excellent Machinability | |
| Bushings for high speed and heavy pressure. | Corrosion Resistance | Corrosion Resistance | |
| Bushings for high speed and heavy pressure. | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bushings for high speed and heavy pressure. | Friction & Wear Properties | Anti-Seizing Properties | |
| Bushings for high speed and heavy pressure. | Friction & Wear Properties | Low Coefficient of Friction | |
| Bushings for high speed and heavy pressure. | Friction & Wear Properties | Wear Resistance | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Corrosion Resistant Castings | Friction & Wear Properties | Wear Resistance | |
| Corrosion Resistant Castings | Machining Properties | Excellent Machinability | |
| Crank Shafts | Corrosion Resistance | Corrosion Resistance | |
| Crank Shafts | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Crank Shafts | Friction & Wear Properties | Anti-Seizing Properties | |
| Crank Shafts | Friction & Wear Properties | Low Coefficient of Friction | |
| Crank Shafts | Friction & Wear Properties | Wear Resistance | |
| Crank Shafts | Machining Properties | Excellent Machinability | |
| High Speed, Heavy Load Bearings | Corrosion Resistance | Corrosion Resistance | |
| High Speed, Heavy Load Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| High Speed, Heavy Load Bearings | Friction & Wear Properties | Anti-Seizing Properties | |
| High Speed, Heavy Load Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| High Speed, Heavy Load Bearings | Friction & Wear Properties | Wear Resistance | |
| High Speed, Heavy Load Bearings | Machining Properties | Excellent Machinability | |
| Impellers | Corrosion Resistance | Corrosion Resistance | |
| Impellers | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Impellers | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Impellers | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Impellers | Friction & Wear Properties | Wear Resistance | |
| Impellers | Machining Properties | Excellent Machinability | |
| Machine Parts | Conductivity (Thermal) | Thermal Conductivity | |
| Machine Parts | Corrosion Resistance | Corrosion Resistance | |
| Machine Parts | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Machine Parts | Friction & Wear Properties | Anti-Seizing Properties | |
| Machine Parts | Friction & Wear Properties | Wear Resistance | |
| Machine Parts | Machining Properties | Excellent Machinability | |
| Parts for Steel Mill Maintenance | Corrosion Resistance | Corrosion Resistance | |
| Parts for Steel Mill Maintenance | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Parts for Steel Mill Maintenance | Friction & Wear Properties | Wear Resistance | |
| Parts for Steel Mill Maintenance | Machining Properties | Excellent Machinability | |
| Parts for Steel Mill Maintenance | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Pressure Tight Castings | Corrosion Resistance | Corrosion Resistance | |
| Pressure Tight Castings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Pressure Tight Castings | Friction & Wear Properties | Wear Resistance | |
| Pressure Tight Castings | Machining Properties | Excellent Machinability | |
| Pressure Tight Castings | Pressure Tight | Pressure Tight to 260 C | |
| Pumps | Corrosion Resistance | Corrosion Resistance | |
| Pumps | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Pumps | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Pumps | Friction & Wear Properties | Anti-Seizing Properties | |
| Pumps | Friction & Wear Properties | Wear Resistance | |
| Slide Guides for Steel Mills | Corrosion Resistance | Corrosion Resistance | |
| Slide Guides for Steel Mills | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Slide Guides for Steel Mills | Friction & Wear Properties | Wear Resistance | |
| Slide Guides for Steel Mills | Machining Properties | Excellent Machinability | |
| Slide Guides for Steel Mills | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Marine | Large Bearings for Ships | Corrosion Resistance | Corrosion Resistance |
| Large Bearings for Ships | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Large Bearings for Ships | Friction & Wear Properties | Anti-Seizing Properties | |
| Large Bearings for Ships | Friction & Wear Properties | Low Coefficient of Friction | |
| Large Bearings for Ships | Friction & Wear Properties | Wear Resistance |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Centrifugal Cast | Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
| Castings | AMS | 4842 | CASTINGS, LEADED BRONZE, SAND AND CENTRIFUGAL, AS CAST | ||
| Castings | SAE | J462 | CAST COPPER ALLOYS | ||
| Castings | ASTM | B271/B271M | COPPER BASE ALLOY CENTRIFUGAL CASTINGS | ||
| As Continuous Cast | Castings | SAE | J462 | CAST COPPER ALLOYS | |
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| Castings | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | ||
| As Sand Cast | Castings | AMS | 4842 | CASTINGS, LEADED BRONZE, SAND AND CENTRIFUGAL, AS CAST | |
| Castings | ASTM | B763/B763M | COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS | ||
| Castings | SAE | J462 | CAST COPPER ALLOYS | ||
| ASTM | B66 | BRONZE CASTINGS IN THE ROUGH FOR LOCOMOTIVE WEARING PARTS | |||
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| Castings | ASTM | B584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | ||
| Castings | ASME | SB584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | ||
| Castings | ASTM | B22/B22M | BRONZE CASTINGS FOR BRIDGES AND TURNTABLES | ||
| Bearings & Busings | AMS | 4827 | BEARINGS, LEADED BRONZE, STEEL BACK | ||
| Ingot | |||||
| ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM |
Corrosion Properties