Find suppliers for this alloyC93700
Chemical Composition
Element
Cu(1)PbSnZnFe(2)P(3)Ni(4)AlSSbSi
(1) Cu + Sum of Named Elements 99.0% min. (2) Fe shall be 0.35% max. when used for steel-backed bearings (3) For continuous castings P shall be 1.5% max. (4) Ni value includes Co.
Min (%)78.08.09.0
Max (%)82.011.011.00.80.70.100.500.0050.080.500.005
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
YS-0.5% Ext
(ksi)
Elongation
(%)
Brinell Hardness, 500 kg load
Shear Strength
(ksi)
Izod
(ft-lbs)
Charpy V-Notch Impact Strength
(ft-lbs)
Compressive Strength .001 in. set/in.
(ksi)
Compressive Strength .1 in. set/in.
(ksi)
Creep Strength (0.1% per 10,000 hours)
(ksi)
Fatigue Strength**
(ksi)
Proportional Limit
(ksi)
As Centrifugal CastAs Centrifugal CastM0230   Min for Standard
30   Min for Standard
12   Min for Standard
12   Min for Standard
15   Min for Standard
15   Min for Standard
As Continuous CastAs Continuous CastM0735   Min for Standard
35   Min for Standard
40   Min for Standard
25   Min for Standard
20   Min for Standard
20   Min for Standard
6   Min for Standard
6   Min for Standard
As Sand CastAs Sand CastM0130   Min for Standard
30   Min for Standard
30   Min for Standard
35   Typ
16   Typ
12   Min for Standard
12   Min for Standard
12   Min for Standard
18   Typ
15   Min for Standard
15   Min for Standard
20   Typ
60   Typ
18   Typ
5   Typ
11   Typ
13   Typ
47   Typ
10   Typ
1.4   Typ
7.4   Typ
13   Typ
8   Typ
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1705
Melting Point - Solidus°F1403
Densitylb/cu in. at 68°F0.32
Specific Gravity8.86
Electrical Conductivity% IACS at 68°F10
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F27.1
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F)10.3
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi11000
Incipient Melting°F600
Magnetic Permeability1
Casting Characteristics

No casting characteristics for this alloy

Fabrication Properties
Technique Suitability Footnote
SolderingGood
BrazingGoodSince brazing is performed in the hot short temperature range, strain must be avoided during brazing and cooling.
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingNot Recommended
Coated Metal Arc WeldingNot Recommended
Machinability Rating80
Common Fabrication Processes
  • Casting
    
Thermal Properties
Treatment Value* Time**
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief500
Solution Treatment0
Typical uses
Product Category Product Reason Category Reason
Builders HardwareBracketsCorrosion ResistanceCorrosion Resistance
BracketsCorrosion ResistanceCorrosion Resistance to Numerous Environments
BracketsMachining PropertiesMachinability, Good
BracketsMechanical PropertiesRelatively Low Strength
FastenersNutsCorrosion ResistanceCorrosion Resistance
NutsCorrosion ResistanceCorrosion Resistance to Numerous Environments
NutsFriction & Wear PropertiesWear Resistance
NutsMachining PropertiesExcellent Machinability
Washers for EnginesCorrosion ResistanceCorrosion Resistance
Washers for EnginesCorrosion ResistanceCorrosion Resistance to Numerous Environments
Washers for EnginesFriction & Wear PropertiesWear Resistance
Washers for EnginesMachining PropertiesExcellent Machinability
IndustrialApplications Requiring Acid Resistance to Sulphite FluidsCorrosion ResistanceCorrosion Resistance
Applications Requiring Acid Resistance to Sulphite FluidsCorrosion ResistanceCorrosion Resistance to Brackish Water
Applications Requiring Acid Resistance to Sulphite FluidsCorrosion ResistanceCorrosion Resistance to Many Industrial Chemicals
Applications Requiring Acid Resistance to Sulphite FluidsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Applications Requiring Acid Resistance to Sulphite FluidsFriction & Wear PropertiesWear Resistance
Applications Requiring Acid Resistance to Sulphite FluidsMachining PropertiesExcellent Machinability
Bearing PlatesCorrosion ResistanceCorrosion Resistance
Bearing PlatesFriction & Wear PropertiesWear Resistance
Bearing PlatesMachining PropertiesMachinability, Good
Bearing PlatesMechanical PropertiesRelatively Low Strength
BearingsCorrosion ResistanceCorrosion Resistance
BearingsCorrosion ResistanceCorrosion Resistance to Numerous Environments
BearingsFriction & Wear PropertiesAnti-Seizing Properties
BearingsFriction & Wear PropertiesLow Coefficient of Friction
BearingsFriction & Wear PropertiesWear Resistance
BearingsMachining PropertiesExcellent Machinability
BushingsCorrosion ResistanceCorrosion Resistance
BushingsCorrosion ResistanceCorrosion Resistance to Numerous Environments
BushingsFriction & Wear PropertiesAnti-Seizing Properties
BushingsFriction & Wear PropertiesLow Coefficient of Friction
BushingsFriction & Wear PropertiesWear Resistance
BushingsMachining PropertiesExcellent Machinability
Bushings for high speed and heavy pressure.Corrosion ResistanceCorrosion Resistance
Bushings for high speed and heavy pressure.Corrosion ResistanceCorrosion Resistance to Numerous Environments
Bushings for high speed and heavy pressure.Friction & Wear PropertiesAnti-Seizing Properties
Bushings for high speed and heavy pressure.Friction & Wear PropertiesLow Coefficient of Friction
Bushings for high speed and heavy pressure.Friction & Wear PropertiesWear Resistance
Corrosion Resistant CastingsCorrosion ResistanceCorrosion Resistance
Corrosion Resistant CastingsCorrosion ResistanceCorrosion Resistance to Brackish Water
Corrosion Resistant CastingsCorrosion ResistanceCorrosion Resistance to Many Industrial Chemicals
Corrosion Resistant CastingsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Corrosion Resistant CastingsFriction & Wear PropertiesWear Resistance
Corrosion Resistant CastingsMachining PropertiesExcellent Machinability
Crank ShaftsCorrosion ResistanceCorrosion Resistance
Crank ShaftsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Crank ShaftsFriction & Wear PropertiesAnti-Seizing Properties
Crank ShaftsFriction & Wear PropertiesLow Coefficient of Friction
Crank ShaftsFriction & Wear PropertiesWear Resistance
Crank ShaftsMachining PropertiesExcellent Machinability
High Speed, Heavy Load BearingsCorrosion ResistanceCorrosion Resistance
High Speed, Heavy Load BearingsCorrosion ResistanceCorrosion Resistance to Numerous Environments
High Speed, Heavy Load BearingsFriction & Wear PropertiesAnti-Seizing Properties
High Speed, Heavy Load BearingsFriction & Wear PropertiesLow Coefficient of Friction
High Speed, Heavy Load BearingsFriction & Wear PropertiesWear Resistance
High Speed, Heavy Load BearingsMachining PropertiesExcellent Machinability
ImpellersCorrosion ResistanceCorrosion Resistance
ImpellersCorrosion ResistanceCorrosion Resistance to Brackish Water
ImpellersCorrosion ResistanceCorrosion Resistance to Many Industrial Chemicals
ImpellersCorrosion ResistanceCorrosion Resistance to Numerous Environments
ImpellersFriction & Wear PropertiesWear Resistance
ImpellersMachining PropertiesExcellent Machinability
Machine PartsConductivity (Thermal)Thermal Conductivity
Machine PartsCorrosion ResistanceCorrosion Resistance
Machine PartsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Machine PartsFriction & Wear PropertiesAnti-Seizing Properties
Machine PartsFriction & Wear PropertiesWear Resistance
Machine PartsMachining PropertiesExcellent Machinability
Parts for Steel Mill MaintenanceCorrosion ResistanceCorrosion Resistance
Parts for Steel Mill MaintenanceCorrosion ResistanceCorrosion Resistance to Numerous Environments
Parts for Steel Mill MaintenanceFriction & Wear PropertiesWear Resistance
Parts for Steel Mill MaintenanceMachining PropertiesExcellent Machinability
Parts for Steel Mill MaintenanceMechanical PropertiesRetains Strength at Elevated Temperatures
Pressure Tight CastingsCorrosion ResistanceCorrosion Resistance
Pressure Tight CastingsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Pressure Tight CastingsFriction & Wear PropertiesWear Resistance
Pressure Tight CastingsMachining PropertiesExcellent Machinability
Pressure Tight CastingsPressure TightPressure Tight to 260 C
PumpsCorrosion ResistanceCorrosion Resistance
PumpsCorrosion ResistanceCorrosion Resistance to Brackish Water
PumpsCorrosion ResistanceCorrosion Resistance to Many Industrial Chemicals
PumpsFriction & Wear PropertiesAnti-Seizing Properties
PumpsFriction & Wear PropertiesWear Resistance
Slide Guides for Steel MillsCorrosion ResistanceCorrosion Resistance
Slide Guides for Steel MillsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Slide Guides for Steel MillsFriction & Wear PropertiesWear Resistance
Slide Guides for Steel MillsMachining PropertiesExcellent Machinability
Slide Guides for Steel MillsMechanical PropertiesRetains Strength at Elevated Temperatures
MarineLarge Bearings for ShipsCorrosion ResistanceCorrosion Resistance
Large Bearings for ShipsCorrosion ResistanceCorrosion Resistance to Salt Water
Large Bearings for ShipsFriction & Wear PropertiesAnti-Seizing Properties
Large Bearings for ShipsFriction & Wear PropertiesLow Coefficient of Friction
Large Bearings for ShipsFriction & Wear PropertiesWear Resistance
Applicable Specifications
Form Sub-Form System Standard Description
As Centrifugal CastCastingsAMS4842CASTINGS, LEADED BRONZE, SAND AND CENTRIFUGAL, AS CAST
CastingsASTMB271/B271MCOPPER BASE ALLOY CENTRIFUGAL CASTINGS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
As Continuous CastCastingsASTMB505/B505MCOPPER BASE ALLOY CONTINUOUS CASTINGS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
As Sand CastCastingsAMS4842CASTINGS, LEADED BRONZE, SAND AND CENTRIFUGAL, AS CAST
CastingsASMESB584COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS
CastingsASTMB22/B22MBRONZE CASTINGS FOR BRIDGES AND TURNTABLES
CastingsASTMB584COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS
ASTMB66BRONZE CASTINGS IN THE ROUGH FOR LOCOMOTIVE WEARING PARTS
CastingsASTMB763/B763MCOPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
Bearings & BusingsAMS4827BEARINGS, LEADED BRONZE, STEEL BACK
Ingot
ASTMB30COPPER BASE ALLOYS IN INGOT FORM
Corrosion Properties

No information available.