| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P(2) | Ni(3) | Al | S | Sb | Si | |
|
(1) Cu + Sum of Named Elements 99.0% min. (2) For continuous castings P shall be 1.5% max. (3) Ni value includes Co. |
|||||||||||
| Min (%) | 75.0 | 13.0 | 6.3 | ||||||||
| Max (%) | 79.0 | 16.0 | 7.5 | 0.8 | 0.15 | 0.05 | 1.0 | 0.005 | 0.08 | 0.8 | 0.005 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load | Shear Strength (ksi) |
Izod (ft-lbs) |
Compressive Strength .001 in. set/in. (ksi) |
Compressive Strength .1 in. set/in. (ksi) |
Fatigue Strength** (ksi) |
Proportional Limit (ksi) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||
| As Centrifugal Cast | As Centrifugal Cast | M02 |
26 Min for Standard 26 Min for Standard 33 Typ |
14 Min for Standard 20 Typ |
12 Min for Standard 12 Min for Standard 12 Typ |
19 Typ | ||||||
| As Continuous Cast | As Continuous Cast | M07 |
25 Min for Standard 25 Min for Standard |
16 Min for Standard |
5 Min for Standard 5 Min for Standard |
|||||||
| As Sand Cast | As Sand Cast | M01 |
26 Min for Standard 26 Min for Standard 30 Typ |
14 Min for Standard 16 Typ |
12 Min for Standard 12 Min for Standard 18 Typ |
55 Typ |
15 Typ |
5 Typ | 12 Typ | 38 Typ | 10 Typ | 4 Typ |
| Melting Point - Liquidus°F | 1730 |
|---|---|
| Melting Point - Solidus°F | 1570 |
| Densitylb/cu in. at 68°F | 0.334 |
| Specific Gravity | 9.25 |
| Electrical Conductivity% IACS at 68°F | 11 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 30.2 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 10.3 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 10500 |
| Incipient Melting°F | 600 |
| Magnetic Permeability | 1 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | High |
| Drossing | Low |
| Effect of Section Size | Low |
| Fluidity | High |
| Gassing | Medium |
| Patternmakers Shrinkage inches per inch | 2/16 |
| Shrinkage in Solidification | Low |
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Poor |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Machinability Rating | 80 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 500 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Acid Resisting Applications | Corrosion Resistance | Corrosion Resistance |
| Acid Resisting Applications | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Acid Resisting Applications | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Acid Resisting Applications | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Acid Resisting Applications | Friction & Wear Properties | Low Coefficient of Friction | |
| Acid Resisting Applications | Friction & Wear Properties | Wear Resistance | |
| Backs for Lined Journal Bearings for Locomotives | Corrosion Resistance | Corrosion Resistance | |
| Backs for Lined Journal Bearings for Locomotives | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Backs for Lined Journal Bearings for Locomotives | Friction & Wear Properties | Low Coefficient of Friction | |
| Backs for Lined Journal Bearings for Locomotives | Friction & Wear Properties | Wear Resistance | |
| Backs for Lined Journal Bearings for Passenger Cars | Corrosion Resistance | Corrosion Resistance | |
| Backs for Lined Journal Bearings for Passenger Cars | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Backs for Lined Journal Bearings for Passenger Cars | Friction & Wear Properties | Low Coefficient of Friction | |
| Backs for Lined Journal Bearings for Passenger Cars | Friction & Wear Properties | Wear Resistance | |
| Bearings | Corrosion Resistance | Corrosion Resistance | |
| Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bearings | Friction & Wear Properties | Anti-Seizing Properties | |
| Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Bearings | Friction & Wear Properties | Wear Resistance | |
| Freight Car Bearings | Corrosion Resistance | Corrosion Resistance | |
| Freight Car Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Freight Car Bearings | Friction & Wear Properties | Anti-Seizing Properties | |
| Freight Car Bearings | Friction & Wear Properties | Low Coefficient of Friction | |
| Freight Car Bearings | Friction & Wear Properties | Wear Resistance | |
| General Service Bearings for Moderate Pressure | Corrosion Resistance | Corrosion Resistance | |
| General Service Bearings for Moderate Pressure | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| General Service Bearings for Moderate Pressure | Friction & Wear Properties | Anti-Seizing Properties | |
| General Service Bearings for Moderate Pressure | Friction & Wear Properties | Low Coefficient of Friction | |
| General Service Bearings for Moderate Pressure | Friction & Wear Properties | Wear Resistance | |
| Industrial Centrifuges | Corrosion Resistance | Corrosion Resistance | |
| Industrial Centrifuges | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Industrial Centrifuges | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Industrial Centrifuges | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Industrial Centrifuges | Friction & Wear Properties | Wear Resistance | |
| Low Friction, Moderate Pressure Bushings | Corrosion Resistance | Corrosion Resistance | |
| Low Friction, Moderate Pressure Bushings | Corrosion Resistance | Corrosion Resistance to Numerous Environmentss | |
| Low Friction, Moderate Pressure Bushings | Friction & Wear Properties | Anti-Seizing Properties | |
| Low Friction, Moderate Pressure Bushings | Friction & Wear Properties | Low Coefficient of Friction | |
| Low Friction, Moderate Pressure Bushings | Friction & Wear Properties | Wear Resistance | |
| Machine Parts | Conductivity (Thermal) | Thermal Conductivity | |
| Machine Parts | Corrosion Resistance | Corrosion Resistance | |
| Machine Parts | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Machine Parts | Friction & Wear Properties | Anti-Seizing Properties | |
| Machine Parts | Friction & Wear Properties | Low Coefficient of Friction | |
| Machine Parts | Friction & Wear Properties | Wear Resistance | |
| Machine Parts | Machining Properties | Excellent Machinability | |
| Pump Bodies for Acid Mine Water | Corrosion Resistance | Corrosion Resistance | |
| Pump Bodies for Acid Mine Water | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Pump Bodies for Acid Mine Water | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Pump Bodies for Acid Mine Water | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Pump Bodies for Acid Mine Water | Friction & Wear Properties | Wear Resistance | |
| Pump Bodies for Acid Mine Water | Machining Properties | Machinability, Good | |
| Pump Impellers for Acid Mine Water | Corrosion Resistance | Corrosion Resistance | |
| Pump Impellers for Acid Mine Water | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Pump Impellers for Acid Mine Water | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Pump Impellers for Acid Mine Water | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Pump Impellers for Acid Mine Water | Friction & Wear Properties | Wear Resistance | |
| Pump Impellers for Acid Mine Water | Machining Properties | Excellent Machinability | |
| Pumps | Corrosion Resistance | Corrosion Resistance | |
| Pumps | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Pumps | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Pumps | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Pumps | Friction & Wear Properties | Low Coefficient of Friction | |
| Pumps | Friction & Wear Properties | Wear Resistance | |
| Railroad Applications | Corrosion Resistance | Corrosion Resistance | |
| Railroad Applications | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Railroad Applications | Friction & Wear Properties | Wear Resistance | |
| Railroad Engine Casings | Conductivity (Thermal) | Thermal Conductivity | |
| Railroad Engine Casings | Corrosion Resistance | Corrosion Resistance | |
| Railroad Engine Casings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Railroad Engine Casings | Friction & Wear Properties | Wear Resistance | |
| Railroad Engine Casings | Pressure Tight | Pressure Tight | |
| Wearing Material for Rod Bushings | Corrosion Resistance | Corrosion Resistance | |
| Wearing Material for Rod Bushings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Wearing Material for Rod Bushings | Friction & Wear Properties | Wear Resistance | |
| Wearing Material for Shoes | Corrosion Resistance | Corrosion Resistance | |
| Wearing Material for Shoes | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Wearing Material for Shoes | Friction & Wear Properties | Wear Resistance | |
| Wearing Material for Wedges | Corrosion Resistance | Corrosion Resistance | |
| Wearing Material for Wedges | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Wearing Material for Wedges | Friction & Wear Properties | Wear Resistance | |
| Marine | Large Bearings for Ships | Corrosion Resistance | Corrosion Resistance |
| Large Bearings for Ships | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Large Bearings for Ships | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Large Bearings for Ships | Friction & Wear Properties | Anti-Seizing Properties | |
| Large Bearings for Ships | Friction & Wear Properties | Low Coefficient of Friction | |
| Large Bearings for Ships | Friction & Wear Properties | Wear Resistance | |
| Large Bearings for Ships | Machining Properties | Machinability, Good |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Centrifugal Cast | Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
| Castings | ASTM | B271/B271M | COPPER BASE ALLOY CENTRIFUGAL CASTINGS | ||
| Castings | SAE | J462 | CAST COPPER ALLOYS | ||
| As Continuous Cast | Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
| Castings | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | ||
| Castings | SAE | J462 | CAST COPPER ALLOYS | ||
| As Permanent Mold Cast | Castings | SAE | J462 | CAST COPPER ALLOYS | |
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| As Sand Cast | MILITARY | MIL-C-22229 | COPPER BASE ALLOY CASTINGS (FOR PRESSURE TIGHT APPLICATIONS) | ||
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| Castings | ASTM | B763/B763M | COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS | ||
| Castings | SAE | J462 | CAST COPPER ALLOYS | ||
| Castings | ASTM | B66 | BRONZE CASTINGS IN THE ROUGH FOR LOCOMOTIVE WEARING PARTS | ||
| Castings | ASTM | B584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | ||
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | ||
Corrosion Properties