Chemical Composition
Element
Cu(1)PbSnZnFeP(2)Ni(3)AlSSbSi
(1) Cu + Sum of Named Elements 99.0% min. (2) For continuous castings P shall be 1.5% max. (3) Ni value includes Co.
Min (%)75.013.06.3
Max (%)79.016.07.50.80.150.051.00.0050.080.80.005
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Brinell Hardness, 500 kg load
Shear Strength
(ksi)
Izod
(ft-lbs)
Compressive Strength .001 in. set/in.
(ksi)
Compressive Strength .1 in. set/in.
(ksi)
Fatigue Strength**
(ksi)
Proportional Limit
(ksi)
As Centrifugal CastAs Centrifugal CastM0226   Min for Standard
26   Min for Standard
33   Typ
14   Min for Standard
14   Min for Standard
20   Typ
12   Min for Standard
12   Min for Standard
12   Typ
19   Typ
As Continuous CastAs Continuous CastM0725   Min for Standard
25   Min for Standard
16   Min for Standard
16   Min for Standard
5   Min for Standard
5   Min for Standard
As Sand CastAs Sand CastM0126   Min for Standard
26   Min for Standard
30   Typ
14   Min for Standard
14   Min for Standard
16   Typ
12   Min for Standard
12   Min for Standard
18   Typ
55   Typ
15   Typ
5   Typ
12   Typ
38   Typ
10   Typ
4   Typ
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1730
Melting Point - Solidus°F1570
Densitylb/cu in. at 68°F0.334
Specific Gravity9.25
Electrical Conductivity% IACS at 68°F11
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F30.2
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F)10.3
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi10500
Incipient Melting°F600
Magnetic Permeability1
Casting Characteristics
Casting Attribute Level
Casting YieldHigh
DrossingLow
Effect of Section SizeLow
FluidityHigh
GassingMedium
Patternmakers Shrinkageinches per inch2/16
Shrinkage in SolidificationLow
Fabrication Properties
Technique Suitability Footnote
SolderingGood
BrazingPoorSince brazing is performed in the hot short temperature range, strain must be avoided during brazing and cooling.
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingNot Recommended
Coated Metal Arc WeldingNot Recommended
Machinability Rating80
Common Fabrication Processes
  • Casting
    
Thermal Properties
Treatment Value* Time**
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief500
Solution Treatment0
Typical uses
Product Category Product Reason Category Reason
IndustrialAcid Resisting ApplicationsCorrosion ResistanceCorrosion Resistance
Acid Resisting ApplicationsCorrosion ResistanceCorrosion Resistance to Brackish Water
Acid Resisting ApplicationsCorrosion ResistanceCorrosion Resistance to Many Industrial Chemicals
Acid Resisting ApplicationsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Acid Resisting ApplicationsFriction & Wear PropertiesLow Coefficient of Friction
Acid Resisting ApplicationsFriction & Wear PropertiesWear Resistance
Backs for Lined Journal Bearings for LocomotivesCorrosion ResistanceCorrosion Resistance
Backs for Lined Journal Bearings for LocomotivesCorrosion ResistanceCorrosion Resistance to Numerous Environments
Backs for Lined Journal Bearings for LocomotivesFriction & Wear PropertiesLow Coefficient of Friction
Backs for Lined Journal Bearings for LocomotivesFriction & Wear PropertiesWear Resistance
Backs for Lined Journal Bearings for Passenger CarsCorrosion ResistanceCorrosion Resistance
Backs for Lined Journal Bearings for Passenger CarsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Backs for Lined Journal Bearings for Passenger CarsFriction & Wear PropertiesLow Coefficient of Friction
Backs for Lined Journal Bearings for Passenger CarsFriction & Wear PropertiesWear Resistance
BearingsCorrosion ResistanceCorrosion Resistance
BearingsCorrosion ResistanceCorrosion Resistance to Numerous Environments
BearingsFriction & Wear PropertiesAnti-Seizing Properties
BearingsFriction & Wear PropertiesLow Coefficient of Friction
BearingsFriction & Wear PropertiesWear Resistance
Freight Car BearingsCorrosion ResistanceCorrosion Resistance
Freight Car BearingsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Freight Car BearingsFriction & Wear PropertiesAnti-Seizing Properties
Freight Car BearingsFriction & Wear PropertiesLow Coefficient of Friction
Freight Car BearingsFriction & Wear PropertiesWear Resistance
General Service Bearings for Moderate PressureCorrosion ResistanceCorrosion Resistance
General Service Bearings for Moderate PressureCorrosion ResistanceCorrosion Resistance to Numerous Environments
General Service Bearings for Moderate PressureFriction & Wear PropertiesAnti-Seizing Properties
General Service Bearings for Moderate PressureFriction & Wear PropertiesLow Coefficient of Friction
General Service Bearings for Moderate PressureFriction & Wear PropertiesWear Resistance
Industrial CentrifugesCorrosion ResistanceCorrosion Resistance
Industrial CentrifugesCorrosion ResistanceCorrosion Resistance to Brackish Water
Industrial CentrifugesCorrosion ResistanceCorrosion Resistance to Many Industrial Chemicals
Industrial CentrifugesCorrosion ResistanceCorrosion Resistance to Numerous Environments
Industrial CentrifugesFriction & Wear PropertiesWear Resistance
Low Friction, Moderate Pressure BushingsCorrosion ResistanceCorrosion Resistance
Low Friction, Moderate Pressure BushingsCorrosion ResistanceCorrosion Resistance to Numerous Environmentss
Low Friction, Moderate Pressure BushingsFriction & Wear PropertiesAnti-Seizing Properties
Low Friction, Moderate Pressure BushingsFriction & Wear PropertiesLow Coefficient of Friction
Low Friction, Moderate Pressure BushingsFriction & Wear PropertiesWear Resistance
Machine PartsConductivity (Thermal)Thermal Conductivity
Machine PartsCorrosion ResistanceCorrosion Resistance
Machine PartsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Machine PartsFriction & Wear PropertiesAnti-Seizing Properties
Machine PartsFriction & Wear PropertiesLow Coefficient of Friction
Machine PartsFriction & Wear PropertiesWear Resistance
Machine PartsMachining PropertiesExcellent Machinability
Pump Bodies for Acid Mine WaterCorrosion ResistanceCorrosion Resistance
Pump Bodies for Acid Mine WaterCorrosion ResistanceCorrosion Resistance to Brackish Water
Pump Bodies for Acid Mine WaterCorrosion ResistanceCorrosion Resistance to Many Industrial Chemicals
Pump Bodies for Acid Mine WaterCorrosion ResistanceCorrosion Resistance to Numerous Environments
Pump Bodies for Acid Mine WaterFriction & Wear PropertiesWear Resistance
Pump Bodies for Acid Mine WaterMachining PropertiesMachinability, Good
Pump Impellers for Acid Mine WaterCorrosion ResistanceCorrosion Resistance
Pump Impellers for Acid Mine WaterCorrosion ResistanceCorrosion Resistance to Brackish Water
Pump Impellers for Acid Mine WaterCorrosion ResistanceCorrosion Resistance to Many Industrial Chemicals
Pump Impellers for Acid Mine WaterCorrosion ResistanceCorrosion Resistance to Numerous Environments
Pump Impellers for Acid Mine WaterFriction & Wear PropertiesWear Resistance
Pump Impellers for Acid Mine WaterMachining PropertiesExcellent Machinability
PumpsCorrosion ResistanceCorrosion Resistance
PumpsCorrosion ResistanceCorrosion Resistance to Brackish Water
PumpsCorrosion ResistanceCorrosion Resistance to Many Industrial Chemicals
PumpsCorrosion ResistanceCorrosion Resistance to Numerous Environments
PumpsFriction & Wear PropertiesLow Coefficient of Friction
PumpsFriction & Wear PropertiesWear Resistance
Railroad ApplicationsCorrosion ResistanceCorrosion Resistance
Railroad ApplicationsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Railroad ApplicationsFriction & Wear PropertiesWear Resistance
Railroad Engine CasingsConductivity (Thermal)Thermal Conductivity
Railroad Engine CasingsCorrosion ResistanceCorrosion Resistance
Railroad Engine CasingsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Railroad Engine CasingsFriction & Wear PropertiesWear Resistance
Railroad Engine CasingsPressure TightPressure Tight
Wearing Material for Rod BushingsCorrosion ResistanceCorrosion Resistance
Wearing Material for Rod BushingsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Wearing Material for Rod BushingsFriction & Wear PropertiesWear Resistance
Wearing Material for ShoesCorrosion ResistanceCorrosion Resistance
Wearing Material for ShoesCorrosion ResistanceCorrosion Resistance to Numerous Environments
Wearing Material for ShoesFriction & Wear PropertiesWear Resistance
Wearing Material for WedgesCorrosion ResistanceCorrosion Resistance
Wearing Material for WedgesCorrosion ResistanceCorrosion Resistance to Numerous Environments
Wearing Material for WedgesFriction & Wear PropertiesWear Resistance
MarineLarge Bearings for ShipsCorrosion ResistanceCorrosion Resistance
Large Bearings for ShipsCorrosion ResistanceCorrosion Resistance to Brackish Water
Large Bearings for ShipsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Large Bearings for ShipsFriction & Wear PropertiesAnti-Seizing Properties
Large Bearings for ShipsFriction & Wear PropertiesLow Coefficient of Friction
Large Bearings for ShipsFriction & Wear PropertiesWear Resistance
Large Bearings for ShipsMachining PropertiesMachinability, Good
Applicable Specifications
Form Sub-Form System Standard Description
As Centrifugal CastCastingsASTMB271/B271MCOPPER BASE ALLOY CENTRIFUGAL CASTINGS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
As Continuous CastCastingsASTMB505/B505MCOPPER BASE ALLOY CONTINUOUS CASTINGS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
As Permanent Mold CastCastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
As Sand CastCastingsASTMB584COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS
CastingsASTMB66BRONZE CASTINGS IN THE ROUGH FOR LOCOMOTIVE WEARING PARTS
CastingsASTMB763/B763MCOPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS
MILITARYMIL-C-22229COPPER BASE ALLOY CASTINGS (FOR PRESSURE TIGHT APPLICATIONS)
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
Ingot
ASTMB30COPPER BASE ALLOYS IN INGOT FORM
Corrosion Properties

No information available.