Find suppliers for this alloy
C94400
| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P(2) | Ni(3) | Al | S | Sb | Si | |
|
(1) Cu + Sum of Named Elements 99.0% min. (2) For continuous castings P shall be 1.5% max. (3) Ni value includes Co. |
|||||||||||
| Min (%) | 9.0 | 7.0 | |||||||||
| Max (%) | Rem | 12.0 | 9.0 | 0.8 | 0.15 | 0.50 | 1.0 | 0.005 | 0.08 | 0.8 | 0.005 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load | Shear Strength (ksi) |
Izod (ft-lbs) |
Compressive Strength .1 in. set/in. (ksi) |
Fatigue Strength** (ksi) |
Proportional Limit (ksi) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | |||||||||||
| As Sand Cast | As Sand Cast | M01 |
32 Typ |
16 Typ |
18 Typ |
55 Typ |
16 Typ |
5 Typ | 44 Typ | 11 Typ | 6 Typ |
| Melting Point - Liquidus°F | 1725 |
|---|---|
| Melting Point - Solidus°F | 1450 |
| Densitylb/cu in. at 68°F | 0.32 |
| Specific Gravity | 8.86 |
| Electrical Conductivity% IACS at 68°F | 10 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 30.2 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 10.3 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 11000 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | High |
| Drossing | Low |
| Effect of Section Size | Low |
| Fluidity | High |
| Gassing | Med-High |
| Patternmakers Shrinkage inches per inch | 2/16 |
| Shrinkage in Solidification | Low |
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Machinability Rating | 80 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 500 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Bearings | Corrosion Resistance | Corrosion Resistance |
| Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bearings | Friction & Wear Properties | Wear Resistance | |
| Bushings | Corrosion Resistance | Corrosion Resistance | |
| Bushings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Corrosion Resistant Castings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Corrosion Resistant Castings | Friction & Wear Properties | Wear Resistance | |
| Floating Rod Bushings | Corrosion Resistance | Corrosion Resistance | |
| Floating Rod Bushings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Floating Rod Bushings | Friction & Wear Properties | Wear Resistance | |
| Locomotive Wear Parts such as Shoes | Conductivity (Thermal) | Thermal Conductivity | |
| Locomotive Wear Parts such as Shoes | Corrosion Resistance | Corrosion Resistance | |
| Locomotive Wear Parts such as Shoes | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Locomotive Wear Parts such as Shoes | Friction & Wear Properties | Wear Resistance | |
| Locomotive Wear Parts such as Wedges | Conductivity (Thermal) | Thermal Conductivity | |
| Locomotive Wear Parts such as Wedges | Corrosion Resistance | Corrosion Resistance | |
| Locomotive Wear Parts such as Wedges | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Locomotive Wear Parts such as Wedges | Friction & Wear Properties | Wear Resistance | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance to Brackish Water | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance to Many Industrial Chemicals | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Pump Impellers | Friction & Wear Properties | Wear Resistance |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Sand Cast | Castings | ASTM | B66 | BRONZE CASTINGS IN THE ROUGH FOR LOCOMOTIVE WEARING PARTS | |
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM |
Corrosion Properties