Find suppliers for this alloyC95200
Chemical Composition
Element
Cu(1)FeAl
(1) Cu + Sum of Named Elements 99.0% min.
Min (%)86.02.58.5
Max (%)4.09.5
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Brinell Hardness, 3000 kg load
Shear Strength
(ksi)
Izod
(ft-lbs)
Charpy V-Notch Impact Strength
(ft-lbs)
Charpy Un-Notched Impact Strength
Compressive Strength .001 in. set/in.
(ksi)
Compressive Strength .1 in. set/in.
(ksi)
Creep Strength (0.1% per 10,000 hours)
(ksi)
Fatigue Strength**
(ksi)
Proportional Limit
(ksi)
As Centrifugal CastAs Centrifugal CastM0265   Min for Standard
65   Min for Standard
65   Min for Standard
25   Min for Standard
25   Min for Standard
25   Min for Standard
20   Min for Standard
20   Min for Standard
110   Min for Standard
As Continuous CastAs Continuous CastM0768   Min for Standard
68   Min for Standard
68   Min for Standard
26   Min for Standard
26   Min for Standard
26   Min for Standard
20   Min for Standard
20   Min for Standard
As Permanent Mold CastAs Permanent Mold CastM0593   Typ
35   Typ
38   Typ
78   Typ
As Sand CastAs Sand CastM0165   Min for Standard
65   Min for Standard
65   Min for Standard
80   Typ
25   Min for Standard
25   Min for Standard
25   Min for Standard
27   Typ
20   Min for Standard
20   Min for Standard
35   Typ
110   Min for Standard
125   Typ
40   Typ
30   Typ
30   Typ
20   Typ
27   Typ
70   Typ
21   Typ
7.9   Typ
22   Typ
12   Typ
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
(1) Field Strength 16000 A/m(200 Oersteds)
Melting Point - Liquidus°F1913
Melting Point - Solidus°F1907
Densitylb/cu in. at 68°F0.276
Specific Gravity7.64
Electrical Conductivity% IACS at 68°F11
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F29.1
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi15000
Magnetic Permeability1.1(1)
Poisson's Ratio0.31
Casting Characteristics
Casting Attribute Level
Casting YieldLow
DrossingHigh
Effect of Section SizeLow
FluidityMedium
GassingMedium
Patternmakers Shrinkageinches per inch4/16
Shrinkage in SolidificationHigh
Shrinkage During FreezingHigh
Fabrication Properties
Technique Suitability
SolderingGood
BrazingGood
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingExcellent
Coated Metal Arc WeldingGood
Machinability Rating20
Common Fabrication Processes
  • Casting
    
Thermal Properties
Treatment Value* Time**
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief600
Solution Treatment0
Typical uses
Product Category Product Reason Category Reason
ElectricalElectrical HardwareConductivity (Thermal)Thermal Conductivity
Electrical HardwareCorrosion ResistanceCorrosion Resistance (Excellent)
Electrical HardwareMechanical PropertiesHigh Strength
FastenersNutsCorrosion ResistanceCorrosion Resistance (Excellent)
NutsMachining PropertiesMachinability, Good
NutsMechanical PropertiesHigh Strength
IndustrialAcid Resistant PumpsCorrosion ResistanceCorrosion Resistance (Excellent)
Acid Resistant PumpsCorrosion ResistanceCorrosion Resistance to Acids
Acid Resistant PumpsCorrosion ResistanceCorrosion Resistance to Fresh Water
Acid Resistant PumpsCorrosion ResistanceCorrosion Resistance to Saline Solutions
Acid Resistant PumpsFriction & Wear PropertiesWear Resistance
Acid Resistant PumpsMachining PropertiesMachinability, Good
Acid Resistant PumpsMechanical PropertiesHigh Strength
Bearing LinersCorrosion ResistanceCorrosion Resistance (Excellent)
Bearing LinersFriction & Wear PropertiesWear Resistance
Bearing LinersMechanical PropertiesHigh Strength
BearingsCorrosion ResistanceCorrosion Resistance (Excellent)
BearingsFriction & Wear PropertiesWear Resistance
BearingsMachining PropertiesMachinability, Good
BearingsMechanical PropertiesHigh Strength
BushingsCorrosion ResistanceCorrosion Resistance (Excellent)
BushingsFriction & Wear PropertiesWear Resistance
BushingsMachining PropertiesMachinability, Good
BushingsMechanical PropertiesHigh Strength
GearsCorrosion ResistanceCorrosion Resistance (Excellent)
GearsFriction & Wear PropertiesWear Resistance
GearsMachining PropertiesMachinability, Good
GearsMechanical PropertiesHigh Strength
High Strength ClampsCorrosion ResistanceCorrosion Resistance
High Strength ClampsMechanical PropertiesHigh Strength
Hot Mill GuidesConductivity (Thermal)Thermal Conductivity
Hot Mill GuidesCorrosion ResistanceCorrosion Resistance (Excellent)
Hot Mill GuidesFriction & Wear PropertiesWear Resistance
Hot Mill GuidesMechanical PropertiesHigh Strength
Hot Mill GuidesMechanical PropertiesRetains Strength at Elevated Temperatures
Hydrant PartsCorrosion ResistanceCorrosion Resistance (Excellent)
Hydrant PartsCorrosion ResistanceCorrosion Resistance to Brackish Water
Hydrant PartsCorrosion ResistanceCorrosion Resistance to Fresh Water
Hydrant PartsFriction & Wear PropertiesWear Resistance
Hydrant PartsMachining PropertiesMachinability, Good
Hydrant PartsMechanical PropertiesHigh Strength
Large Gear PartsCorrosion ResistanceCorrosion Resistance (Excellent)
Large Gear PartsFriction & Wear PropertiesWear Resistance
Large Gear PartsMechanical PropertiesHigh Strength
Mild Alkali ApplicationsCorrosion ResistanceCorrosion Resistance (Excellent)
Mild Alkali ApplicationsCorrosion ResistanceCorrosion Resistance to Acids
Mild Alkali ApplicationsFriction & Wear PropertiesWear Resistance
Mild Alkali ApplicationsMechanical PropertiesHigh Strength
Pickling EquipmentCorrosion ResistanceCorrosion Resistance (Excellent)
Pickling EquipmentCorrosion ResistanceCorrosion Resistance to Acids
Pickling EquipmentMachining PropertiesMachinability, Good
Pickling EquipmentMechanical PropertiesHigh Strength
Pickling TanksCorrosion ResistanceCorrosion Resistance (Excellent)
Pickling TanksCorrosion ResistanceCorrosion Resistance to Acids
Pickling TanksFriction & Wear PropertiesWear Resistance
Pickling TanksMechanical PropertiesHigh Strength
PlungersCorrosion ResistanceCorrosion Resistance (Excellent)
PlungersFriction & Wear PropertiesWear Resistance
PlungersMachining PropertiesMachinability, Good
PlungersMechanical PropertiesHigh Strength
Pump PartsCorrosion ResistanceCorrosion Resistance (Excellent)
Pump PartsCorrosion ResistanceCorrosion Resistance to Acids
Pump PartsCorrosion ResistanceCorrosion Resistance to Fresh Water
Pump PartsCorrosion ResistanceCorrosion Resistance to Saline Solutions
Pump PartsFriction & Wear PropertiesWear Resistance
Pump PartsMachining PropertiesMachinability, Good
Pump PartsMechanical PropertiesHigh Strength
Pump RodsCorrosion ResistanceCorrosion Resistance (Excellent)
Pump RodsFriction & Wear PropertiesWear Resistance
Pump RodsMachining PropertiesMachinability, Good
Pump RodsMechanical PropertiesHigh Strength
Thrust PadsCorrosion ResistanceCorrosion Resistance (Excellent)
Thrust PadsFriction & Wear PropertiesWear Resistance
Thrust PadsMechanical PropertiesHigh Strength
Valve BodiesCorrosion ResistanceCorrosion Resistance (Excellent)
Valve BodiesFriction & Wear PropertiesWear Resistance
Valve BodiesMachining PropertiesMachinability, Good
Valve BodiesMechanical PropertiesHigh Strength
Valve SeatsCorrosion ResistanceCorrosion Resistance
Valve SeatsCorrosion ResistanceCorrosion Resistance (Excellent)
Valve SeatsFriction & Wear PropertiesWear Resistance
Valve SeatsMachining PropertiesMachinability, Good
Valve SeatsMechanical PropertiesHigh Strength
ValvesCorrosion ResistanceCorrosion Resistance (Excellent)
ValvesFriction & Wear PropertiesWear Resistance
ValvesMachining PropertiesMachinability, Good
ValvesMechanical PropertiesHigh Strength
Wear PlatesCorrosion ResistanceCorrosion Resistance (Excellent)
Wear PlatesFriction & Wear PropertiesWear Resistance
Wear PlatesMechanical PropertiesHigh Strength
Welding JawsConductivity (Thermal)Thermal Conductivity
Welding JawsCorrosion ResistanceCorrosion Resistance (Excellent)
Welding JawsMechanical PropertiesHigh Strength
Welding JawsMechanical PropertiesRetains Strength at Elevated Temperatures
Worm WheelsCorrosion ResistanceCorrosion Resistance (Excellent)
Worm WheelsFriction & Wear PropertiesWear Resistance
Worm WheelsMachining PropertiesMachinability, Good
Worm WheelsMechanical PropertiesHigh Strength
WormsCorrosion ResistanceCorrosion Resistance (Excellent)
WormsFriction & Wear PropertiesWear Resistance
WormsMachining PropertiesMachinability, Good
WormsMechanical PropertiesHigh Strength
MarineCovers for Marine HardwareAppearanceAppearance
Covers for Marine HardwareCorrosion ResistanceCorrosion Resistance (Excellent)
Covers for Marine HardwareCorrosion ResistanceCorrosion Resistance to Fresh Water
Covers for Marine HardwareCorrosion ResistanceCorrosion Resistance to Salt Water
Covers for Marine HardwareMechanical PropertiesHigh Strength
Marine EnginesCorrosion ResistanceCorrosion Resistance (Excellent)
Marine EnginesCorrosion ResistanceCorrosion Resistance to Brackish Water
Marine EnginesCorrosion ResistanceCorrosion Resistance to Fresh Water
Marine EnginesFriction & Wear PropertiesWear Resistance
Marine EnginesMechanical PropertiesFatigue Properties
Marine EnginesMechanical PropertiesHigh Strength
Marine HardwareCorrosion ResistanceCorrosion Resistance (Excellent)
Marine HardwareCorrosion ResistanceCorrosion Resistance to Fresh Water
Marine HardwareCorrosion ResistanceCorrosion Resistance to Saline Solutions
Marine HardwareMechanical PropertiesHigh Strength
PropellersCorrosion ResistanceCorrosion Resistance (Excellent)
PropellersCorrosion ResistanceCorrosion Resistance to Brackish Water
PropellersCorrosion ResistanceCorrosion Resistance to Fresh Water
PropellersFriction & Wear PropertiesWear Resistance
PropellersMechanical PropertiesHigh Strength
PropellersMechanical PropertiesRetains Strength at Elevated Temperatures
OrdnanceGun MountingsCorrosion ResistanceCorrosion Resistance (Excellent)
Gun MountingsFriction & Wear PropertiesWear Resistance
Gun MountingsMechanical PropertiesHigh Strength
Gun SlidesCorrosion ResistanceCorrosion Resistance (Excellent)
Gun SlidesFriction & Wear PropertiesWear Resistance
Gun SlidesMechanical PropertiesHigh Strength
Applicable Specifications
Form Sub-Form System Standard Description
As Centrifugal CastCastingsASMESB271COPPER BASE ALLOY CENTRIFUGAL CASTINGS
CastingsASTMB271/B271MCOPPER BASE ALLOY CENTRIFUGAL CASTINGS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
As Continuous CastCastingsASMESB505COPPER BASE ALLOY CONTINUOUS CASTINGS
CastingsASTMB505/B505MCOPPER BASE ALLOY CONTINUOUS CASTINGS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
As Sand CastCastingsASMESB148ALUMINUM BRONZE SAND CASTINGS
CastingsASTMB148ALUMINUM BRONZE SAND CASTINGS
CastingsASTMB763/B763MCOPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
FlangesASMEB16.24BRONZE PIPE FLANGES AND FLANGED FITTINGS
ASMESB148ALUMINUM BRONZE SAND CASTINGS
ASTMB148ALUMINUM BRONZE SAND CASTINGS
Ingot
ASTMB30COPPER BASE ALLOYS IN INGOT FORM
Valves
Corrosion Properties

No information available.