Find suppliers for this alloy
C95400
| Elements | |||||
|---|---|---|---|---|---|
| Cu(1) | Fe | Ni(2) | Al | Mn | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co. |
|||||
| Min (%) | 83.0 | 3.0 | 10.0 | ||
| Max (%) | 5.0 | 1.5 | 11.5 | 0.50 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 3000 kg load | Shear Strength (ksi) |
Izod (ft-lbs) |
Charpy V-Notch Impact Strength (ft-lbs) |
Charpy Un-Notched Impact Strength | Compressive Strength .1 in. set/in. (ksi) |
Creep Strength (0.1% per 10,000 hours) (ksi) |
Fatigue Strength** (ksi) |
Proportional Limit (ksi) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||||
| As Centrifugal Cast | As Centrifugal Cast | M02 |
75 Min for Standard 75 Min for Standard |
30 Min for Standard |
12 Min for Standard 12 Min for Standard |
150 Min for Standard |
||||||||
| Quenched Hardened and Temper Annealed | TQ50 |
90 Min for Standard 90 Min for Standard |
6 Min for Standard 6 Min for Standard |
190 Min for Standard |
||||||||||
| As Continuous Cast | As Continuous Cast | M07 |
85 Min for Standard 85 Min for Standard |
32 Min for Standard |
12 Min for Standard 12 Min for Standard |
|||||||||
| Quenched Hardened and Temper Annealed | TQ50 |
95 Min for Standard 95 Min for Standard |
10 Min for Standard 10 Min for Standard |
|||||||||||
| As Permanent Mold Cast | As Permanent Mold Cast | M05 |
100 Min for Standard 105 Typ |
40 Min for Standard 46 Typ |
10 Min for Standard 11 Typ |
|||||||||
| As Sand Cast | As Sand Cast | M01 |
75 Min for Standard |
30 Min for Standard |
12 Min for Standard |
150 Min for Standard |
||||||||
| As Sand Cast | M01 |
75 Min for Standard 75 Min for Standard 85 Typ |
35 Typ |
12 Min for Standard 12 Min for Standard 18 Typ |
150 Min for Standard 170 Typ |
47 Typ |
11 Typ | 100 Typ | 7.4 Typ | 28 Typ | 17 Typ | |||
| Quenched Hardened and Temper Annealed | TQ50 |
90 Min |
6 Min |
190 Min |
||||||||||
| Quenched Hardened and Temper Annealed | TQ50 |
90 Min for Standard 90 Min for Standard 105 Typ |
54 Typ |
6 Min for Standard 6 Min for Standard 8 Typ |
190 Min for Standard 195 Typ |
50 Typ |
11 Typ | 7 Typ | 120 Typ | 35 Typ | 28 Typ | |||
| (1)As Cast, Field Strength 16 kA/m(2)TQ 50 Temper, Field Sterngth 16 kA/m | |
| Melting Point - Liquidus°F | 1900 |
|---|---|
| Melting Point - Solidus°F | 1880 |
| Densitylb/cu in. at 68°F | 0.269 |
| Specific Gravity | 7.45 |
| Electrical Conductivity% IACS at 68°F | 13 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 33.9 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.1 |
| Modulus of Elasticity in Tensionksi | 15500 |
| Magnetic Permeability | 1.27 (1) |
| Magnetic Permeability | 1.2 (2) |
| Casting Attribute | Level |
|---|---|
| Casting Yield | Low |
| Drossing | High |
| Effect of Section Size | Low |
| Fluidity | Medium |
| Gassing | Medium |
| Patternmakers Shrinkage inches per inch | 3/16 |
| Shrinkage in Solidification | High |
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Good |
| Machinability Rating | 60 |
Common Fabrication Processes
| Treatment | Minimum* | Maximum* | Value* | Time** | Medium |
|---|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | |||||
| Stress Relief | 600 | ||||
| Solution Treatment | 1600 | 1675 | 1 | Water | |
| Annealing | 1150 | 1225 | 1 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Automotive | Weld Guns | Conductivity (Thermal) | Thermal Conductivity |
| Weld Guns | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Weld Guns | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Weld Guns | Friction & Wear Properties | Wear Resistance | |
| Weld Guns | Machining Properties | Machinability, Good | |
| Weld Guns | Mechanical Properties | High Strength | |
| Weld Guns | Mechanical Properties | Moderate Strength | |
| Weld Guns | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Fasteners | Large Hold Down Screws | Corrosion Resistance | Corrosion Resistance (Excellent) |
| Large Hold Down Screws | Machining Properties | Machinability, Good | |
| Large Hold Down Screws | Mechanical Properties | High Strength | |
| Nuts | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Nuts | Mechanical Properties | High Strength | |
| Industrial | Bearing Segments for the Steel Industry | Corrosion Resistance | Corrosion Resistance (Excellent) |
| Bearing Segments for the Steel Industry | Friction & Wear Properties | Wear Resistance | |
| Bearing Segments for the Steel Industry | Mechanical Properties | High Strength | |
| Bearing Segments for the Steel Industry | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Bearing Segments for the Steel Industry | Mechanical Properties | Toughness | |
| Bearings | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Bearings | Friction & Wear Properties | Wear Resistance | |
| Bearings | Mechanical Properties | High Strength | |
| Bearings | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Bearings | Mechanical Properties | Toughness | |
| Bushings | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Bushings | Machining Properties | Machinability, Good | |
| Bushings | Mechanical Properties | High Strength | |
| Gears | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Gears | Friction & Wear Properties | Wear Resistance | |
| Gears | Machining Characteristics | Excellent Machinability | |
| Gears | Mechanical Properties | High Strength | |
| Heavily Loaded Worm Gears | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Heavily Loaded Worm Gears | Friction & Wear Properties | Wear Resistance | |
| Heavily Loaded Worm Gears | Machining Properties | Machinability, Good | |
| Heavily Loaded Worm Gears | Mechanical Properties | High Strength | |
| High Strength Clamps | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| High Strength Clamps | Mechanical Properties | High Strength | |
| Landing Gear Parts | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Landing Gear Parts | Friction & Wear Properties | Wear Resistance | |
| Landing Gear Parts | Mechanical Properties | Fatigue Properties | |
| Landing Gear Parts | Mechanical Properties | High Strength | |
| Machine Parts | Conductivity (Thermal) | Thermal Conductivity | |
| Machine Parts | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Machine Parts | Friction & Wear Properties | Wear Resistance | |
| Machine Parts | Machining Characteristics | Excellent Machinability | |
| Machine Parts | Mechanical Properties | High Strength | |
| Machine Parts | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Pawl | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Pawl | Friction & Wear Properties | Wear Resistance | |
| Pawl | Mechanical Properties | High Strength | |
| Pickling Hooks | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Pickling Hooks | Corrosion Resistance | Corrosion Resistance to Acids | |
| Pickling Hooks | Friction & Wear Properties | Wear Resistance | |
| Pickling Hooks | Mechanical Properties | High Strength | |
| Pressure Blocks for the Steel Industry | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Pressure Blocks for the Steel Industry | Friction & Wear Properties | Wear Resistance | |
| Pressure Blocks for the Steel Industry | Mechanical Properties | High Strength | |
| Pressure Blocks for the Steel Industry | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Pump Parts | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Pump Parts | Friction & Wear Properties | Wear Resistance | |
| Pump Parts | Machining Properties | Machinability, Good | |
| Pump Parts | Mechanical Properties | High Strength | |
| Spur Gears | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Spur Gears | Friction & Wear Properties | Wear Resistance | |
| Spur Gears | Mechanical Properties | High Strength | |
| Valve Bodies | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Valve Bodies | Friction & Wear Properties | Wear Resistance | |
| Valve Bodies | Machining Properties | Machinability, Good | |
| Valve Bodies | Mechanical Properties | High Strength | |
| Valve Guides | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Valve Guides | Friction & Wear Properties | Wear Resistance | |
| Valve Guides | Mechanical Properties | High Strength | |
| Valve Seats | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Valve Seats | Friction & Wear Properties | Wear Resistance | |
| Valve Seats | Machining Characteristics | Excellent Machinability | |
| Valve Seats | Mechanical Properties | High Strength | |
| Valves | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Valves | Friction & Wear Properties | Wear Resistance | |
| Valves | Machining Properties | Machinability, Good | |
| Valves | Mechanical Properties | High Strength | |
| Worm Gears | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Worm Gears | Friction & Wear Properties | Wear Resistance | |
| Worm Gears | Machining Properties | Machinability, Good | |
| Worm Gears | Mechanical Properties | High Strength | |
| Marine | Covers for Marine Hardware | Appearance | Appearance |
| Covers for Marine Hardware | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Covers for Marine Hardware | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Covers for Marine Hardware | Mechanical Properties | High Strength | |
| Ship Building | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Ship Building | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Ship Building | Friction & Wear Properties | Wear Resistance | |
| Ship Building | Mechanical Properties | High Strength | |
| Ordnance | Government Fittings | Corrosion Resistance | Corrosion Resistance (Excellent) |
| Government Fittings | Friction & Wear Properties | Wear Resistance | |
| Government Fittings | Machining Characteristics | Excellent Machinability | |
| Government Fittings | Mechanical Properties | High Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Centrifugal Cast | Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
| Castings | ASTM | B271/B271M | COPPER BASE ALLOY CENTRIFUGAL CASTINGS | ||
| Castings | SAE | J462 | CAST COPPER ALLOYS | ||
| Castings | ASME | SB271 | COPPER BASE ALLOY CENTRIFUGAL CASTINGS | ||
| As Continuous Cast | Castings | SAE | J462 | CAST COPPER ALLOYS | |
| Castings | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | ||
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| As Permanent Mold Cast | Castings | ASTM | B806 | PERMANENT MOLD CASTINGS | |
| As Sand Cast | Castings | SAE | J462 | CAST COPPER ALLOYS | |
| Castings | ASTM | B148 | ALUMINUM BRONZE SAND CASTINGS | ||
| Castings | ASTM | B763/B763M | COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS | ||
| Castings | ASME | SB148 | ALUMINUM BRONZE SAND CASTINGS | ||
| Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| ASTM | B66 | BRONZE CASTINGS IN THE ROUGH FOR LOCOMOTIVE WEARING PARTS | |||
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | ||
| Precision Cast | Castings | MILITARY | MIL-C-11866 | CASTINGS, PRECISION, NONFERROUS |
Corrosion Properties