Chemical Composition
Element
Cu(1)FeNi(2)AlMn
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co.
Min (%)83.03.010.0
Max (%)5.01.511.50.50
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Brinell Hardness, 3000 kg load
Shear Strength
(ksi)
Izod
(ft-lbs)
Charpy V-Notch Impact Strength
(ft-lbs)
Charpy Un-Notched Impact Strength
Compressive Strength .1 in. set/in.
(ksi)
Creep Strength (0.1% per 10,000 hours)
(ksi)
Fatigue Strength**
(ksi)
Proportional Limit
(ksi)
As Centrifugal CastAs Centrifugal CastM0275   Min for Standard
75   Min for Standard
75   Min for Standard
30   Min for Standard
30   Min for Standard
30   Min for Standard
12   Min for Standard
12   Min for Standard
150   Min for Standard
Quenched Hardened and Temper AnnealedTQ5090   Min for Standard
90   Min for Standard
45   Min for Standard
45   Min for Standard
6   Min for Standard
6   Min for Standard
190   Min for Standard
As Continuous CastAs Continuous CastM0785   Min for Standard
85   Min for Standard
32   Min for Standard
32   Min for Standard
12   Min for Standard
12   Min for Standard
Quenched Hardened and Temper AnnealedTQ5095   Min for Standard
95   Min for Standard
45   Min for Standard
45   Min for Standard
10   Min for Standard
10   Min for Standard
As Permanent Mold CastAs Permanent Mold CastM05100   Min for Standard
105   Typ
40   Min for Standard
46   Typ
10   Min for Standard
11   Typ
As Sand CastAs Sand CastM0175   Min for Standard
75   Min for Standard
30   Min for Standard
30   Min for Standard
12   Min for Standard
150   Min for Standard
M0175   Min for Standard
75   Min for Standard
75   Min for Standard
85   Typ
30   Min for Standard
30   Min for Standard
30   Min for Standard
35   Typ
12   Min for Standard
12   Min for Standard
18   Typ
150   Min for Standard
170   Typ
47   Typ
16   Typ
11   Typ
100   Typ
7.4   Typ
2.9   Typ
17   Typ
4.4   Typ
28   Typ
17   Typ
Quenched Hardened and Temper AnnealedTQ5090   Min
45   Min
6   Min
190   Min
TQ5090   Min for Standard
90   Min for Standard
105   Typ
45   Min for Standard
45   Min for Standard
54   Typ
6   Min for Standard
6   Min for Standard
8   Typ
190   Min for Standard
195   Typ
50   Typ
11   Typ
7   Typ
120   Typ
35   Typ
28   Typ
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
(1) As Cast, Field Strength 16 kA/m
(2) TQ 50 Temper, Field Sterngth 16 kA/m
Melting Point - Liquidus°F1900
Melting Point - Solidus°F1880
Densitylb/cu in. at 68°F0.269
Specific Gravity7.45
Electrical Conductivity% IACS at 68°F13
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F33.9
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9
Specific Heat CapacityBtu/ lb /°F at 68°F0.1
Modulus of Elasticity in Tensionksi15500
Magnetic Permeability1.27(1)
Magnetic Permeability1.2(2)
Casting Characteristics
Casting Attribute Level
Casting YieldLow
DrossingHigh
Effect of Section SizeLow
FluidityMedium
GassingMedium
Patternmakers Shrinkageinches per inch3/16
Shrinkage in SolidificationHigh
Fabrication Properties
Technique Suitability
SolderingGood
BrazingGood
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingGood
Machinability Rating60
Common Fabrication Processes
  • Casting
    
Thermal Properties
Treatment Minimum* Maximum* Value* Time** Medium
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief600
Solution Treatment160016751Water
Annealing115012251
Typical uses
Product Category Product Reason Category Reason
AutomotiveWeld GunsConductivity (Thermal)Thermal Conductivity
Weld GunsCorrosion ResistanceCorrosion Resistance (Excellent)
Weld GunsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Weld GunsFriction & Wear PropertiesWear Resistance
Weld GunsMachining PropertiesMachinability, Good
Weld GunsMechanical PropertiesHigh Strength
Weld GunsMechanical PropertiesModerate Strength
Weld GunsMechanical PropertiesRetains Strength at Elevated Temperatures
FastenersLarge Hold Down ScrewsCorrosion ResistanceCorrosion Resistance (Excellent)
Large Hold Down ScrewsMachining PropertiesMachinability, Good
Large Hold Down ScrewsMechanical PropertiesHigh Strength
NutsCorrosion ResistanceCorrosion Resistance (Excellent)
NutsMechanical PropertiesHigh Strength
IndustrialBearing Segments for the Steel IndustryCorrosion ResistanceCorrosion Resistance (Excellent)
Bearing Segments for the Steel IndustryFriction & Wear PropertiesWear Resistance
Bearing Segments for the Steel IndustryMechanical PropertiesHigh Strength
Bearing Segments for the Steel IndustryMechanical PropertiesRetains Strength at Elevated Temperatures
Bearing Segments for the Steel IndustryMechanical PropertiesToughness
BearingsCorrosion ResistanceCorrosion Resistance (Excellent)
BearingsFriction & Wear PropertiesWear Resistance
BearingsMechanical PropertiesHigh Strength
BearingsMechanical PropertiesRetains Strength at Elevated Temperatures
BearingsMechanical PropertiesToughness
BushingsCorrosion ResistanceCorrosion Resistance (Excellent)
BushingsFriction & Wear PropertiesWear Resistance
BushingsMachining PropertiesMachinability, Good
BushingsMechanical PropertiesHigh Strength
GearsCorrosion ResistanceCorrosion Resistance (Excellent)
GearsFriction & Wear PropertiesWear Resistance
GearsMachining CharacteristicsExcellent Machinability
GearsMechanical PropertiesHigh Strength
Heavily Loaded Worm GearsCorrosion ResistanceCorrosion Resistance (Excellent)
Heavily Loaded Worm GearsFriction & Wear PropertiesWear Resistance
Heavily Loaded Worm GearsMachining PropertiesMachinability, Good
Heavily Loaded Worm GearsMechanical PropertiesHigh Strength
High Strength ClampsCorrosion ResistanceCorrosion Resistance (Excellent)
High Strength ClampsMechanical PropertiesHigh Strength
Landing Gear PartsCorrosion ResistanceCorrosion Resistance (Excellent)
Landing Gear PartsFriction & Wear PropertiesWear Resistance
Landing Gear PartsMechanical PropertiesFatigue Properties
Landing Gear PartsMechanical PropertiesHigh Strength
Machine PartsConductivity (Thermal)Thermal Conductivity
Machine PartsCorrosion ResistanceCorrosion Resistance (Excellent)
Machine PartsFriction & Wear PropertiesWear Resistance
Machine PartsMachining CharacteristicsExcellent Machinability
Machine PartsMechanical PropertiesHigh Strength
Machine PartsMechanical PropertiesRetains Strength at Elevated Temperatures
PawlCorrosion ResistanceCorrosion Resistance (Excellent)
PawlFriction & Wear PropertiesWear Resistance
PawlMechanical PropertiesHigh Strength
Pickling HooksCorrosion ResistanceCorrosion Resistance (Excellent)
Pickling HooksCorrosion ResistanceCorrosion Resistance to Acids
Pickling HooksFriction & Wear PropertiesWear Resistance
Pickling HooksMechanical PropertiesHigh Strength
Pressure Blocks for the Steel IndustryCorrosion ResistanceCorrosion Resistance (Excellent)
Pressure Blocks for the Steel IndustryFriction & Wear PropertiesWear Resistance
Pressure Blocks for the Steel IndustryMechanical PropertiesHigh Strength
Pressure Blocks for the Steel IndustryMechanical PropertiesRetains Strength at Elevated Temperatures
Pump PartsCorrosion ResistanceCorrosion Resistance (Excellent)
Pump PartsFriction & Wear PropertiesWear Resistance
Pump PartsMachining PropertiesMachinability, Good
Pump PartsMechanical PropertiesHigh Strength
Spur GearsCorrosion ResistanceCorrosion Resistance (Excellent)
Spur GearsFriction & Wear PropertiesWear Resistance
Spur GearsMechanical PropertiesHigh Strength
Valve BodiesCorrosion ResistanceCorrosion Resistance (Excellent)
Valve BodiesFriction & Wear PropertiesWear Resistance
Valve BodiesMachining PropertiesMachinability, Good
Valve BodiesMechanical PropertiesHigh Strength
Valve GuidesCorrosion ResistanceCorrosion Resistance (Excellent)
Valve GuidesFriction & Wear PropertiesWear Resistance
Valve GuidesMechanical PropertiesHigh Strength
Valve SeatsCorrosion ResistanceCorrosion Resistance (Excellent)
Valve SeatsFriction & Wear PropertiesWear Resistance
Valve SeatsMachining CharacteristicsExcellent Machinability
Valve SeatsMechanical PropertiesHigh Strength
ValvesCorrosion ResistanceCorrosion Resistance (Excellent)
ValvesFriction & Wear PropertiesWear Resistance
ValvesMachining PropertiesMachinability, Good
ValvesMechanical PropertiesHigh Strength
Worm GearsCorrosion ResistanceCorrosion Resistance (Excellent)
Worm GearsFriction & Wear PropertiesWear Resistance
Worm GearsMachining PropertiesMachinability, Good
Worm GearsMechanical PropertiesHigh Strength
MarineCovers for Marine HardwareAppearanceAppearance
Covers for Marine HardwareCorrosion ResistanceCorrosion Resistance (Excellent)
Covers for Marine HardwareCorrosion ResistanceCorrosion Resistance to Salt Water
Covers for Marine HardwareMechanical PropertiesHigh Strength
Ship BuildingCorrosion ResistanceCorrosion Resistance (Excellent)
Ship BuildingCorrosion ResistanceCorrosion Resistance to Salt Water
Ship BuildingFriction & Wear PropertiesWear Resistance
Ship BuildingMechanical PropertiesHigh Strength
OrdnanceGovernment FittingsCorrosion ResistanceCorrosion Resistance (Excellent)
Government FittingsFriction & Wear PropertiesWear Resistance
Government FittingsMachining CharacteristicsExcellent Machinability
Government FittingsMechanical PropertiesHigh Strength
Applicable Specifications
Form Sub-Form System Standard Description
As Centrifugal CastCastingsASMESB271COPPER BASE ALLOY CENTRIFUGAL CASTINGS
CastingsASTMB271/B271MCOPPER BASE ALLOY CENTRIFUGAL CASTINGS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
As Continuous CastCastingsASTMB505/B505MCOPPER BASE ALLOY CONTINUOUS CASTINGS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
As Permanent Mold CastCastingsASTMB806PERMANENT MOLD CASTINGS
As Sand CastCastingsASMESB148ALUMINUM BRONZE SAND CASTINGS
CastingsASTMB148ALUMINUM BRONZE SAND CASTINGS
ASTMB66BRONZE CASTINGS IN THE ROUGH FOR LOCOMOTIVE WEARING PARTS
CastingsASTMB763/B763MCOPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
IngotASTMB30COPPER BASE ALLOYS IN INGOT FORM
Precision CastCastingsMILITARYMIL-C-11866CASTINGS, PRECISION, NONFERROUS
Corrosion Properties

No information available.