Find suppliers for this alloy
C95410
| Elements | |||||
|---|---|---|---|---|---|
| Cu(1) | Fe | Ni(2) | Al | Mn | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co. |
|||||
| Min (%) | 83.0 | 3.0 | 1.5 | 10.0 | |
| Max (%) | 5.0 | 2.5 | 11.5 | 0.50 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 3000 kg load | Shear Strength (ksi) |
Izod (ft-lbs) |
Compressive Strength .1 in. set/in. (ksi) |
Creep Strength (0.1% per 10,000 hours) (ksi) |
Fatigue Strength** (ksi) |
Proportional Limit (ksi) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||
| As Centrifugal Cast | As Centrifugal Cast | M02 |
75 Min for Standard |
30 Min for Standard |
12 Min for Standard |
150 Min for Standard |
||||||
| Quenched Hardened and Temper Annealed | TQ50 |
90 Min for Standard |
6 Min for Standard |
190 Min for Standard |
||||||||
| As Continuous Cast | As Continuous Cast | M07 |
85 Min for Standard |
32 Min for Standard |
12 Min for Standard |
|||||||
| Quenched Hardened and Temper Annealed | TQ50 |
95 Min for Standard |
10 Min for Standard |
|||||||||
| As Permanent Mold Cast | As Permanent Mold Cast | M05 |
100 Min for Standard |
40 Min for Standard |
10 Min for Standard |
|||||||
| As Sand Cast | As Sand Cast | M01 |
75 Min for Standard 85 Typ |
30 Min for Standard 35 Typ |
12 Min for Standard 18 Typ |
150 Min for Standard 170 Typ |
47 Typ |
14 Typ | 100 Typ | 4 Typ | 28 Typ | 17 Typ |
| Quenched Hardened and Temper Annealed | TQ50 |
90 Min for Standard 105 Typ |
54 Typ |
6 Min for Standard 8 Typ |
190 Min for Standard 195 Typ |
50 Typ |
120 Typ | 35 Typ | 28 Typ | |||
| Melting Point - Liquidus°F | 1900 |
|---|---|
| Melting Point - Solidus°F | 1880 |
| Densitylb/cu in. at 68°F | 0.269 |
| Specific Gravity | 7.45 |
| Electrical Conductivity% IACS at 68°F | 13 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 33.9 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.1 |
| Modulus of Elasticity in Tensionksi | 15500 |
Casting Characteristics
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Good |
| Machinability Rating | 60 |
Common Fabrication Processes
| Treatment | Minimum* | Maximum* | Value* | Time** | Medium |
|---|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | |||||
| Stress Relief | 600 | ||||
| Solution Treatment | 1600 | 1675 | 1 | Water | |
| Annealing | 1150 | 1225 | 1 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Bearings | Corrosion Resistance | Corrosion Resistance |
| Bearings | Friction & Wear Properties | Wear Resistance | |
| Bearings | Mechanical Properties | Fatigue Strength | |
| Bearings | Mechanical Properties | High Strength | |
| Bearings | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Bushings | Corrosion Resistance | Corrosion Resistance | |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Bushings | Mechanical Properties | Fatigue Strength | |
| Bushings | Mechanical Properties | High Strength | |
| Bushings | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Gears | Corrosion Resistance | Corrosion Resistance | |
| Gears | Friction & Wear Properties | Wear Resistance | |
| Gears | Mechanical Properties | Fatigue Strength | |
| Gears | Mechanical Properties | High Strength | |
| Gears | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Pickling Baskets | Corrosion Resistance | Corrosion Resistance | |
| Pickling Baskets | Corrosion Resistance | Corrosion Resistance to Acids | |
| Pickling Baskets | Friction & Wear Properties | Wear Resistance | |
| Pickling Baskets | Mechanical Properties | High Strength | |
| Pickling Baskets | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Pickling Hooks | Corrosion Resistance | Corrosion Resistance | |
| Pickling Hooks | Friction & Wear Properties | Wear Resistance | |
| Pickling Hooks | Mechanical Properties | Fatigue Strength | |
| Pickling Hooks | Mechanical Properties | High Strength | |
| Pickling Hooks | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Spur Gears | Corrosion Resistance | Corrosion Resistance | |
| Spur Gears | Friction & Wear Properties | Wear Resistance | |
| Spur Gears | Mechanical Properties | Fatigue Strength | |
| Spur Gears | Mechanical Properties | High Strength | |
| Spur Gears | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Valve Components | Corrosion Resistance | Corrosion Resistance | |
| Valve Components | Friction & Wear Properties | Wear Resistance | |
| Valve Components | Mechanical Properties | Fatigue Strength | |
| Valve Components | Mechanical Properties | High Strength | |
| Valve Components | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Worms | Corrosion Resistance | Corrosion Resistance | |
| Worms | Corrosion Resistance | Corrosion Resistance to Acids | |
| Worms | Friction & Wear Properties | Wear Resistance | |
| Worms | Mechanical Properties | Fatigue Strength | |
| Worms | Mechanical Properties | High Strength | |
| Worms | Mechanical Properties | Retains Strength at Elevated Temperatures |
Applicable Specifications
Corrosion Properties