Chemical Composition
Element
Cu(1)FeNi(2)AlMn
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co.
Min (%)78.03.03.010.0
Max (%)5.05.511.53.5
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Brinell Hardness, 3000 kg load
Shear Strength
(ksi)
Izod
(ft-lbs)
Charpy V-Notch Impact Strength
(ft-lbs)
Compressive Strength .1 in. set/in.
(ksi)
Creep Strength (0.1% per 10,000 hours)
(ksi)
Fatigue Strength**
(ksi)
Proportional Limit
(ksi)
As Centrifugal CastAs Centrifugal CastM0290   Min for Standard
90   Min for Standard
40   Min for Standard
40   Min for Standard
6   Min for Standard
6   Min for Standard
190   Min for Standard
Quenched Hardened and Temper AnnealedTQ50110   Min for Standard
110   Min for Standard
60   Min for Standard
60   Min for Standard
5   Min for Standard
5   Min for Standard
200   Min for Standard
As Continuous CastAs Continuous CastM0795   Min for Standard
95   Min for Standard
42   Min for Standard
42   Min for Standard
10   Min for Standard
10   Min for Standard
Quenched Hardened and Temper AnnealedTQ50110   Min for Standard
110   Min for Standard
62   Min for Standard
62   Min for Standard
8   Min for Standard
8   Min for Standard
As Permanent Mold CastAs Permanent Mold CastM05110   Min for Standard
60   Min for Standard
5   Min for Standard
As Sand CastAs Sand CastM0190   Min for Standard
90   Min for Standard
100   Typ
40   Min for Standard
40   Min for Standard
44   Typ
6   Min for Standard
6   Min for Standard
12   Typ
87   Typ
190   Min for Standard
195   Typ
48   Typ
13   Typ
10   Typ
120   Typ
11   Typ
3   Typ
6   Typ
31   Typ
28   Typ
Quenched Hardened and Temper AnnealedTQ50110   Min for Standard
110   Min for Standard
120   Typ
60   Min for Standard
60   Min for Standard
68   Typ
5   Min for Standard
5   Min for Standard
10   Typ
200   Min for Standard
230   Typ
70   Typ
15   Typ
150   Typ
38   Typ
45   Typ
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
(1) As Cast, Field Strength 16 kA/m
(2) TQ 50 Temper, Field Strength 16 kA/m
Melting Point - Liquidus°F1930
Melting Point - Solidus°F1900
Densitylb/cu in. at 68°F0.272
Specific Gravity7.53
Electrical Conductivity% IACS at 68°F8
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F24.2
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9
Specific Heat CapacityBtu/ lb /°F at 68°F0.1
Modulus of Elasticity in Tensionksi16000
Magnetic Permeability1.32(1)
Magnetic Permeability1.2(2)
Poisson's Ratio0.32
Casting Characteristics
Casting Attribute Level
Casting YieldLow
DrossingHigh
Effect of Section SizeLow
FluidityMedium
GassingMedium
Patternmakers Shrinkageinches per inch3/16
Shrinkage in SolidificationHigh
Fabrication Properties
Technique Suitability
SolderingGood
BrazingFair
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingGood
Machinability Rating50
Common Fabrication Processes
  • Casting
    
Thermal Properties
Treatment Minimum* Maximum* Value* Time** Medium
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief600
Solution Treatment160016751Water
Annealing115012251
Typical uses
Product Category Product Reason Category Reason
Builders HardwareWindow HardwareAppearanceAppearance
Window HardwareCorrosion ResistanceCorrosion Resistance (Excellent)
Window HardwareMachining CharacteristicsExcellent Machinability
Window HardwareMechanical PropertiesHigh Strength
ConsumerMusical InstrumentsAppearanceAppearance
Musical InstrumentsCorrosion ResistanceCorrosion Resistance (Excellent)
Musical InstrumentsDamping CharacteristicsResonant Frequency, Damping Capacity
Musical InstrumentsFriction & Wear PropertiesWear Resistance
Musical InstrumentsMachining CharacteristicsExcellent Machinability
Musical InstrumentsMechanical PropertiesHigh Strength
Piano KeysAppearanceAppearance
Piano KeysCorrosion ResistanceCorrosion Resistance (Excellent)
Piano KeysFriction & Wear PropertiesWear Resistance
Piano KeysMachining CharacteristicsExcellent Machinability
Piano KeysMechanical PropertiesHigh Strength
ElectricalElectrical HardwareConductivity (Electrical)Electrical Conductivity
Electrical HardwareConductivity (Thermal)Thermal Conductivity
Electrical HardwareCorrosion ResistanceCorrosion Resistance (Excellent)
Electrical HardwareMechanical PropertiesHigh Strength
FastenersStuffing Box NutsCorrosion ResistanceCorrosion Resistance (Excellent)
Stuffing Box NutsFriction & Wear PropertiesWear Resistance
Stuffing Box NutsMechanical PropertiesHigh Strength
IndustrialAir Craft ComponentsCorrosion ResistanceCorrosion Resistance (Excellent)
Air Craft ComponentsFriction & Wear PropertiesWear Resistance
Air Craft ComponentsMechanical PropertiesHigh Strength
Air Craft ComponentsMechanical PropertiesRetains Strength at Elevated Temperatures
Air Craft ComponentsMechanical PropertiesToughness
BearingsCorrosion ResistanceCorrosion Resistance (Excellent)
BearingsFriction & Wear PropertiesWear Resistance
BearingsMechanical PropertiesHigh Strength
BushingsCorrosion ResistanceCorrosion Resistance (Excellent)
BushingsFriction & Wear PropertiesWear Resistance
BushingsMechanical PropertiesHigh Strength
GearsCorrosion ResistanceCorrosion Resistance (Excellent)
GearsFriction & Wear PropertiesWear Resistance
GearsMechanical PropertiesHigh Strength
GlandsCorrosion ResistanceCorrosion Resistance (Excellent)
GlandsFriction & Wear PropertiesWear Resistance
GlandsMechanical PropertiesHigh Strength
Glass MoldsCorrosion ResistanceCorrosion Resistance (Excellent)
Glass MoldsFriction & Wear PropertiesWear Resistance
Glass MoldsMechanical PropertiesHigh Strength
Glass MoldsMechanical PropertiesRetains Strength at Elevated Temperatures
Hand Gun Recoil MechanismsCorrosion ResistanceCorrosion Resistance (Excellent)
Hand Gun Recoil MechanismsMechanical PropertiesHigh Strength
Hand Gun Recoil MechanismsMechanical PropertiesToughness
Hot Mill GuidesCorrosion ResistanceCorrosion Resistance (Excellent)
Hot Mill GuidesMechanical PropertiesHigh Strength
Hot Mill GuidesMechanical PropertiesRetains Strength at Elevated Temperatures
Hot Mill GuidesMechanical PropertiesToughness
Landing Gear PartsCorrosion ResistanceCorrosion Resistance
Landing Gear PartsCorrosion ResistanceCorrosion Resistance (Excellent)
Landing Gear PartsFriction & Wear PropertiesWear Resistance
Landing Gear PartsFriction & Wear PropertiesWear Resistance
Landing Gear PartsMechanical PropertiesFatigue Properties
Landing Gear PartsMechanical PropertiesFatigue Strength
Landing Gear PartsMechanical PropertiesHigh Strength
Landing Gear PartsMechanical PropertiesHigh Strength
Landing Gear PartsMechanical PropertiesRetains Strength at Elevated Temperatures
Machine PartsConductivity (Thermal)Thermal Conductivity
Machine PartsCorrosion ResistanceCorrosion Resistance (Excellent)
Machine PartsFriction & Wear PropertiesWear Resistance
Machine PartsMachining CharacteristicsExcellent Machinability
Machine PartsMechanical PropertiesHigh Strength
Pickling EquipmentCorrosion ResistanceCorrosion Resistance (Excellent)
Pickling EquipmentCorrosion ResistanceCorrosion Resistance to Acids
Pickling EquipmentMechanical PropertiesHigh Strength
Piston GuidesCorrosion ResistanceCorrosion Resistance (Excellent)
Piston GuidesFriction & Wear PropertiesWear Resistance
Piston GuidesMechanical PropertiesHigh Strength
Pump Fluid EndsCorrosion ResistanceCorrosion Resistance (Excellent)
Pump Fluid EndsMechanical PropertiesHigh Strength
Sewage Treatment ApplicationsCorrosion ResistanceCorrosion Resistance (Excellent)
Sewage Treatment ApplicationsFriction & Wear PropertiesWear Resistance
Sewage Treatment ApplicationsMechanical PropertiesHigh Strength
Valve BodiesCorrosion ResistanceCorrosion Resistance (Excellent)
Valve BodiesMachining CharacteristicsExcellent Machinability
Valve BodiesMechanical PropertiesHigh Strength
Valve ComponentsCorrosion ResistanceCorrosion Resistance (Excellent)
Valve ComponentsFriction & Wear PropertiesWear Resistance
Valve ComponentsMechanical PropertiesHigh Strength
Valve GuidesCorrosion ResistanceCorrosion Resistance (Excellent)
Valve GuidesFriction & Wear PropertiesWear Resistance
Valve GuidesMechanical PropertiesHigh Strength
Valve SeatsCorrosion ResistanceCorrosion Resistance (Excellent)
Valve SeatsFriction & Wear PropertiesWear Resistance
Valve SeatsMechanical PropertiesHigh Strength
Wear PlatesCorrosion ResistanceCorrosion Resistance (Excellent)
Wear PlatesFriction & Wear PropertiesWear Resistance
Wear PlatesMechanical PropertiesToughness
Welding JawsConductivity (Thermal)Thermal Conductivity
Welding JawsCorrosion ResistanceCorrosion Resistance (Excellent)
Welding JawsMechanical PropertiesHigh Strength
Welding JawsMechanical PropertiesRetains Strength at Elevated Temperatures
Welding JawsMechanical PropertiesToughness
WormsCorrosion ResistanceCorrosion Resistance (Excellent)
WormsFriction & Wear PropertiesWear Resistance
WormsMachining PropertiesMachinability, Good
WormsMechanical PropertiesHigh Strength
Worms WheelsCorrosion ResistanceCorrosion Resistance (Excellent)
Worms WheelsFriction & Wear PropertiesWear Resistance
Worms WheelsMechanical PropertiesHigh Strength
MarineCovers for Marine HardwareAppearanceAppearance
Covers for Marine HardwareCorrosion ResistanceCorrosion Resistance (Excellent)
Covers for Marine HardwareCorrosion ResistanceCorrosion Resistance to Salt Water
Covers for Marine HardwareMechanical PropertiesHigh Strength
Marine ApplicationsCorrosion ResistanceCorrosion Resistance (Excellent)
Marine ApplicationsCorrosion ResistanceCorrosion Resistance to Salt Water
Marine ApplicationsFriction & Wear PropertiesWear Resistance
Marine ApplicationsMechanical PropertiesHigh Strength
Marine HardwareAppearanceAppearance
Marine HardwareCorrosion ResistanceCorrosion Resistance (Excellent)
Marine HardwareCorrosion ResistanceCorrosion Resistance to Salt Water
Marine HardwareMechanical PropertiesHigh Strength
Ship BuildingCorrosion ResistanceCorrosion Resistance (Excellent)
Ship BuildingFriction & Wear PropertiesWear Resistance
Ship BuildingMachining PropertiesMachinability, Good
Ship BuildingMechanical PropertiesHigh Strength
OrdnanceGovernment FittingsCorrosion ResistanceCorrosion Resistance (Excellent)
Government FittingsMechanical PropertiesHigh Strength
Government FittingsMechanical PropertiesToughness
Applicable Specifications
Form Sub-Form System Standard Description
As Centrifugal CastCastingsASTMB271/B271MCOPPER BASE ALLOY CENTRIFUGAL CASTINGS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
As Continuous CastCastingsASTMB505/B505MCOPPER BASE ALLOY CONTINUOUS CASTINGS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
As Sand CastCastingsASTMB148ALUMINUM BRONZE SAND CASTINGS
CastingsASTMB763/B763MCOPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
Ingot
ASTMB30COPPER BASE ALLOYS IN INGOT FORM
Precision CastCastingsASTMB806PERMANENT MOLD CASTINGS
Valves
Corrosion Properties

No information available.