Find suppliers for this alloy
C95700
| Elements | ||||||
|---|---|---|---|---|---|---|
| Cu(1) | Fe | Ni(2) | Al | Mn | Si | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co. |
||||||
| Min (%) | 71.0 | 2.0 | 1.5 | 7.0 | 11.0 | |
| Max (%) | 4.0 | 3.0 | 8.5 | 14.0 | 0.10 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell C scale | Brinell Hardness, 3000 kg load | Stress Rupture (ksi) |
Izod (ft-lbs) |
Charpy V-Notch Impact Strength (ft-lbs) |
Compressive Strength .1 in. set/in. (ksi) |
Creep Strength (0.1% per 10,000 hours) (ksi) |
Fatigue Strength** (ksi) |
Proportional Limit (ksi) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||||
| As Continuous Cast | As Continuous Cast | M07 |
90 Min for Standard |
40 Min for Standard |
15 Min for Standard |
|||||||||
| As Permanent Mold Cast | As Permanent Mold Cast | M05 | 1 Typ |
|||||||||||
| As Permanent Mold Cast | M05 |
129 Typ |
75 Typ |
25 Typ |
||||||||||
| As Permanent Mold Cast | M05 |
90 Min for Standard |
15 Min for Standard |
|||||||||||
| As Sand Cast | As Sand Cast | M01 |
90 Min for Standard 95 Typ |
40 Min for Standard 45 Typ |
20 Min for Standard 26 Typ |
180 Typ |
34 Typ | 25 Typ | 30 Typ |
150 Typ | 9.6 Typ | 33 Typ | 22 Typ | |
| (1)Annealed, Fast Cooled Condition(2)Slow Cooled Condition, Range 2.2 to 15.0 | |
| Melting Point - Liquidus°F | 1814 |
|---|---|
| Melting Point - Solidus°F | 1742 |
| Densitylb/cu in. at 68°F | 0.272 |
| Specific Gravity | 7.53 |
| Electrical Conductivity% IACS at 68°F | 3 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 7 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.8 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.105 |
| Modulus of Elasticity in Tensionksi | 18000 |
| Magnetic Permeability | 1.03 (1) |
| Magnetic Permeability | 2.2 (2) |
| Poisson's Ratio | 0.326 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | Low |
| Drossing | High |
| Effect of Section Size | Low |
| Fluidity | Medium |
| Gassing | Medium |
| Patternmakers Shrinkage inches per inch | 3/16 |
| Shrinkage in Solidification | High |
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Excellent |
| Coated Metal Arc Welding | Good |
| Machinability Rating | 50 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 600 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Consumer | Safety Tools | Corrosion Resistance | Corrosion Resistance (Excellent) |
| Safety Tools | Mechanical Properties | High Strength | |
| Safety Tools | Non-Magnetic | Non-Magnetic | |
| Safety Tools | Non-Sparking | Non-Sparking | |
| Fasteners | Nuts | Corrosion Resistance | Corrosion Resistance (Excellent) |
| Nuts | Mechanical Properties | High Strength | |
| Stator Clamps | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Stator Clamps | Mechanical Properties | Fatigue Strength | |
| Stator Clamps | Mechanical Properties | High Strength | |
| Industrial | Bushings | Corrosion Resistance | Corrosion Resistance (Excellent) |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Bushings | Mechanical Properties | High Strength | |
| Gears | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Gears | Friction & Wear Properties | Wear Resistance | |
| Gears | Mechanical Properties | High Strength | |
| Hot Mill Guides | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Hot Mill Guides | Friction & Wear Properties | Wear Resistance | |
| Hot Mill Guides | Mechanical Properties | High Strength | |
| Hot Mill Guides | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Impellers | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Impellers | Friction & Wear Properties | Wear Resistance | |
| Impellers | Mechanical Properties | High Strength | |
| Pickling Equipment | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Pickling Equipment | Corrosion Resistance | Corrosion Resistance to Acids | |
| Pickling Equipment | Mechanical Properties | High Strength | |
| Propellers | Corrosion Resistance | Corrosion Resistance | |
| Propellers | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Propellers | Friction & Wear Properties | Wear Resistance | |
| Propellers | Friction & Wear Properties | Wear Resistance | |
| Propellers | Mechanical Properties | Fatigue Strength | |
| Propellers | Mechanical Properties | Fatigue Strength | |
| Propellers | Mechanical Properties | High Strength | |
| Propellers | Mechanical Properties | High Strength | |
| Pump Casings | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Pump Casings | Friction & Wear Properties | Wear Resistance | |
| Pump Casings | Machining Properties | Machinability, Good | |
| Pump Casings | Mechanical Properties | High Strength | |
| Pump Castings | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Pump Castings | Friction & Wear Properties | Wear Resistance | |
| Pump Castings | Machining Properties | Machinability, Good | |
| Pump Castings | Mechanical Properties | High Strength | |
| Stator Clamp Segments | Corrosion Resistance | Corrosion Resistance | |
| Stator Clamp Segments | Friction & Wear Properties | Wear Resistance | |
| Stator Clamp Segments | Mechanical Properties | Fatigue Strength | |
| Stator Clamp Segments | Mechanical Properties | High Strength | |
| Valves | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Valves | Friction & Wear Properties | Wear Resistance | |
| Valves | Mechanical Properties | High Strength | |
| Wear Plates | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Wear Plates | Friction & Wear Properties | Wear Resistance | |
| Wear Plates | Mechanical Properties | High Strength | |
| Welding Rods | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Welding Rods | Mechanical Properties | High Strength | |
| Worm Wheels | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Worm Wheels | Friction & Wear Properties | Wear Resistance | |
| Worm Wheels | Mechanical Properties | High Strength | |
| Worms | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Worms | Friction & Wear Properties | Wear Resistance | |
| Worms | Mechanical Properties | High Strength | |
| Marine | Marine Hardware | Appearance | Appearance |
| Marine Hardware | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Marine Hardware | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Marine Hardware | Mechanical Properties | High Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Continuous Cast | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | ||
| As Sand Cast | Castings | ASTM | B148 | ALUMINUM BRONZE SAND CASTINGS | |
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | ||
Corrosion Properties