Find suppliers for this alloyC95800
Chemical Composition
Element
Cu(1)PbFe(2)Ni(3)AlMnSi
(1) Cu + Sum of Named Elements 99.5% min. (2) Fe content shall not exceed Ni content. (3) Fe content shall not exceed Ni content.
Min (%)79.03.54.08.50.8
Max (%)0.034.55.09.51.50.10
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Brinell Hardness, 3000 kg load
Shear Strength
(ksi)
Izod
(ft-lbs)
Charpy V-Notch Impact Strength
(ft-lbs)
Compressive Strength .001 in. set/in.
(ksi)
Compressive Strength .01 in. set/in.
(ksi)
Compressive Strength .1 in. set/in.
(ksi)
Fatigue Strength**
(ksi)
As Centrifugal CastAs Centrifugal CastM0285   Min for Standard
85   Min for Standard
35   Min for Standard
35   Min for Standard
15   Min for Standard
15   Min for Standard
As Continuous CastAs Continuous CastM0785   Min for Standard
85   Min for Standard
35   Min for Standard
35   Min for Standard
18   Min for Standard
18   Min for Standard
As Permanent Mold CastAs Permanent Mold CastM0590   Min for Standard
96   Typ
40   Min for Standard
52   Typ
15   Min for Standard
17   Typ
88   Typ
As Sand CastAs Sand CastM0185   Min for Standard
85   Min for Standard
95   Typ
35   Min for Standard
35   Min for Standard
38   Typ
15   Min for Standard
15   Min for Standard
25   Typ
159   Typ
58   Typ
20   Typ
10   Typ
16   Typ
35   Typ
48   Typ
100   Typ
31   Typ
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
(1) Field Sterength 16 kA/m
Melting Point - Liquidus°F1940
Melting Point - Solidus°F1910
Densitylb/cu in. at 68°F0.276
Specific Gravity7.64
Electrical Conductivity% IACS at 68°F7
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F20.8
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9
Specific Heat CapacityBtu/ lb /°F at 68°F0.105
Modulus of Elasticity in Tensionksi16500
Magnetic Permeability1.05(1)
Poisson's Ratio0.32
Casting Characteristics
Casting Attribute Level
Casting YieldLow
DrossingHigh
Effect of Section SizeLow
FluidityMedium
GassingMedium
Patternmakers Shrinkageinches per inch3/16
Shrinkage in SolidificationHigh
Fabrication Properties
Technique Suitability
SolderingGood
BrazingFair
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingGood
Machinability Rating20
Common Fabrication Processes
  • Casting
    
Thermal Properties
Treatment Value* Time**
* Temperature is measured in Fahrenheit. ** Time is measured in minutes.
Stress Relief600
Solution Treatment0
Typical uses
Product Category Product Reason Category Reason
FastenersNutsCorrosion ResistanceCorrosion Resistance (Excellent)
NutsMachining PropertiesMachinability, Good
NutsMechanical PropertiesHigh Strength
IndustrialBushingsCorrosion ResistanceCorrosion Resistance (Excellent)
BushingsFriction & Wear PropertiesWear Resistance
BushingsMachining PropertiesMachinability, Good
BushingsMechanical PropertiesHigh Strength
GearsCorrosion ResistanceCorrosion Resistance (Excellent)
GearsFriction & Wear PropertiesWear Resistance
GearsMachining PropertiesMachinability, Good
GearsMechanical PropertiesHigh Strength
MachineryConductivity (Thermal)Thermal Conductivity
MachineryCorrosion ResistanceCorrosion Resistance (Excellent)
MachineryFriction & Wear PropertiesWear Resistance
MachineryMechanical PropertiesHigh Strength
Pickling EquipmentCorrosion ResistanceCorrosion Resistance (Excellent)
Pickling EquipmentCorrosion ResistanceCorrosion Resistance to Acids
Pickling EquipmentMechanical PropertiesHigh Strength
Propeller BladesCorrosion ResistanceCorrosion Resistance (Excellent)
Propeller BladesFriction & Wear PropertiesWear Resistance
Propeller BladesMechanical PropertiesFatigue Strength
Propeller BladesMechanical PropertiesHigh Strength
Propeller HubCorrosion ResistanceCorrosion Resistance (Excellent)
Propeller HubFriction & Wear PropertiesWear Resistance
Propeller HubMechanical PropertiesFatigue Strength
Propeller HubMechanical PropertiesHigh Strength
ShaftsCorrosion ResistanceCorrosion Resistance (Excellent)
ShaftsFriction & Wear PropertiesWear Resistance
ShaftsMechanical PropertiesHigh Strength
Valve BodiesCorrosion ResistanceCorrosion Resistance (Excellent)
Valve BodiesFriction & Wear PropertiesWear Resistance
Valve BodiesMechanical PropertiesHigh Strength
Wear PlatesCorrosion ResistanceCorrosion Resistance (Excellent)
Wear PlatesFriction & Wear PropertiesWear Resistance
Wear PlatesMechanical PropertiesHigh Strength
Worm WheelsCorrosion ResistanceCorrosion Resistance (Excellent)
Worm WheelsFriction & Wear PropertiesWear Resistance
Worm WheelsMachining PropertiesMachinability, Good
Worm WheelsMechanical PropertiesHigh Strength
WormsCorrosion ResistanceCorrosion Resistance (Excellent)
WormsFriction & Wear PropertiesWear Resistance
WormsMechanical PropertiesHigh Strength
MarineCovers for Marine HardwareAppearanceAppearance
Covers for Marine HardwareCorrosion ResistanceCorrosion Resistance (Excellent)
Covers for Marine HardwareCorrosion ResistanceCorrosion Resistance to Saline Solutions
Covers for Marine HardwareCorrosion ResistanceCorrosion Resistance to Salt Water
Covers for Marine HardwareMechanical PropertiesHigh Strength
Marine HardwareAppearanceAppearance
Marine HardwareCorrosion ResistanceCorrosion Resistance (Excellent)
Marine HardwareCorrosion ResistanceCorrosion Resistance to Fresh Water
Marine HardwareCorrosion ResistanceCorrosion Resistance to Saline Solutions
Marine HardwareMechanical PropertiesHigh Strength
Ship BuildingCorrosion ResistanceCorrosion Resistance (Excellent)
Ship BuildingCorrosion ResistanceCorrosion Resistance to Saline Solutions
Ship BuildingCorrosion ResistanceCorrosion Resistance to Salt Water
Ship BuildingFriction & Wear PropertiesWear Resistance
Ship BuildingMechanical PropertiesHigh Strength
Valves in contact with sea water.Corrosion ResistanceCorrosion Resistance (Excellent)
Valves in contact with sea water.Corrosion ResistanceCorrosion Resistance to Fresh Water
Valves in contact with sea water.Corrosion ResistanceCorrosion Resistance to Saline Solutions
Valves in contact with sea water.Friction & Wear PropertiesWear Resistance
Valves in contact with sea water.Mechanical PropertiesHigh Strength
PlumbingElbowsCorrosion ResistanceCorrosion Resistance (Excellent)
ElbowsMachining PropertiesMachinability, Good
ElbowsMechanical PropertiesHigh Strength
ElbowsMechanical PropertiesRetains Strength at Elevated Temperatures
Applicable Specifications
Form Sub-Form System Standard Description
As Centrifugal CastCastingsASTMB271/B271MCOPPER BASE ALLOY CENTRIFUGAL CASTINGS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
As Continuous CastCastingsASTMB505/B505MCOPPER BASE ALLOY CONTINUOUS CASTINGS
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
As Sand CastCastingsASTMB148ALUMINUM BRONZE SAND CASTINGS
CastingsASTMB763/B763MCOPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS
CastingsMILITARYMIL-B-24480BRONZE, NICKEL-ALUMINUM CASTINGS, FOR SEAWATER SERVICE
CastingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
CastingsSAEJ462CAST COPPER ALLOYS
Ingot
ASTMB30COPPER BASE ALLOYS IN INGOT FORM
Precision CastCastingsASTMB806PERMANENT MOLD CASTINGS
Valves