C95815
Elements | ||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|
Cu(1) | Pb | Sn | Zn | Fe | Ni | Al | Bi | Cr | Mg | Mn | Si | |
(1) Cu + Sum of Named Elements 99.5% min. |
||||||||||||
Min (%) | 76.0 | 4.0 | 4.0 | 8.8 | ||||||||
Max (%) | 82.5 | 0.03 | 0.10 | 0.40 | 5.5 | 5.3 | 10.0 | 0.01 | 0.05 | 0.05 | 2.5 | 0.10 |
Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Brinell Hardness, 3000 kg load |
---|---|---|---|---|---|---|
* Measured at room temperature, 68°F (20°C). | ||||||
As Centrifugal Cast | As Centrifugal Cast | M02 |
94.3 Min |
40 Min |
||
As Centrifugal Cast | M02 |
94.3 Min |
40.6 Min |
13 Min |
150 Min |
|
As Permanent Mold Cast | As Permanent Mold Cast | M05 |
94.3 Min |
40.6 Min |
7 Min |
150 Min |
As Sand Cast | As Sand Cast | M01 |
87.0 Min |
36.3 Min |
13 Min |
140 Min |
Physical Properties
Casting Characteristics
Fabrication Properties
Common Fabrication Processes
Typical Uses
Applicable Specifications
Corrosion Properties