Find suppliers for this alloy
C96200
| Elements | ||||||||||
|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Fe | P | Ni(2) | C | Mn | S | Si | Nb(3) | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co. (3) When product or casting is intended for subsequent welding applications, and so specified by the purchaser the Nb content shall be 0.40% max. |
||||||||||
| Min (%) | 1.0 | 9.0 | ||||||||
| Max (%) | Rem | 0.01 | 1.8 | 0.02 | 11.0 | 0.10 | 1.5 | 0.02 | 0.50 | 1.0 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
Elongation (%) |
Charpy V-Notch Impact Strength (ft-lbs) |
Compressive Strength .1 in. set/in. (ksi) |
Fatigue Strength** (ksi) |
|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | |||||||
| As Sand Cast | As Sand Cast | M01 |
45 Min |
20 Min |
100 Typ |
37 Typ | 13 Typ |
| Melting Point - Liquidus°F | 2100 |
|---|---|
| Melting Point - Solidus°F | 2010 |
| Densitylb/cu in. at 68°F | 0.323 |
| Specific Gravity | 8.94 |
| Electrical Conductivity% IACS at 68°F | 11 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 26.1 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.5 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 18000 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | Low |
| Drossing | Low |
| Effect of Section Size | Low |
| Fluidity | High |
| Gassing | High |
| Patternmakers Shrinkage inches per inch | 3/16 |
| Shrinkage in Solidification | High |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Poor |
| Coated Metal Arc Welding | Fair |
| Machinability Rating | 10 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 0 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Chemical Processing Equipment | Corrosion Resistance | Corrosion Resistance (Excellent) |
| Chemical Processing Equipment | Corrosion Resistance | Erosion and Impingement Resistance | |
| Chemical Processing Equipment | Mechanical Properties | High Strength | |
| Chemical Processing Equipment | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Components for Oil Refineries | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Components for Oil Refineries | Corrosion Resistance | Erosion and Impingement Resistance | |
| Components for Oil Refineries | Mechanical Properties | High Strength | |
| Components for Oil Refineries | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Fittings | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Fittings | Mechanical Properties | High Strength | |
| Steam Fittings | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Steam Fittings | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Steam Fittings | Mechanical Properties | High Strength | |
| Steam Fittings | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Marine | Component Parts for Sea Water Corrosion Resistance. | Corrosion Resistance | Corrosion Resistance (Excellent) |
| Component Parts for Sea Water Corrosion Resistance. | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Component Parts for Sea Water Corrosion Resistance. | Corrosion Resistance | Erosion and Impingement Resistance | |
| Component Parts for Sea Water Corrosion Resistance. | Mechanical Properties | High Strength | |
| Elbows to Resist Sea Water | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Elbows to Resist Sea Water | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Elbows to Resist Sea Water | Mechanical Properties | High Strength | |
| Flanges to Resist Sea Water | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Flanges to Resist Sea Water | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Flanges to Resist Sea Water | Mechanical Properties | High Strength | |
| Propeller Sleeves to Resist Sea Water | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Propeller Sleeves to Resist Sea Water | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Propeller Sleeves to Resist Sea Water | Corrosion Resistance | Erosion and Impingement Resistance | |
| Propeller Sleeves to Resist Sea Water | Mechanical Properties | High Strength | |
| Pump Bodies to Resist Sea Water | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Pump Bodies to Resist Sea Water | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Pump Bodies to Resist Sea Water | Mechanical Properties | High Strength | |
| Pump Impellers to Resist Sea Water | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Pump Impellers to Resist Sea Water | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Pump Impellers to Resist Sea Water | Corrosion Resistance | Erosion and Impingement Resistance | |
| Pump Impellers to Resist Sea Water | Mechanical Properties | High Strength | |
| Valves to Resist Sea Water | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Valves to Resist Sea Water | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Valves to Resist Sea Water | Corrosion Resistance | Erosion and Impingement Resistance | |
| Valves to Resist Sea Water | Mechanical Properties | High Strength | |
| Plumbing | Plumbing Parts | Corrosion Resistance | Corrosion Resistance (Excellent) |
| Plumbing Parts | Corrosion Resistance | Erosion and Impingement Resistance | |
| Plumbing Parts | Mechanical Properties | High Strength | |
| Plumbing Parts | Mechanical Properties | Retains Strength at Elevated Temperatures |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Centrifugal Cast | Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
| Castings | SAE | J462 | CAST COPPER ALLOYS | ||
| As Sand Cast | Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
| Castings | SAE | J462 | CAST COPPER ALLOYS | ||
| Castings | Copper-Nickel Alloy | ASTM | B369 | COPPER NICKEL ALLOY CASTINGS | |
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | ||
| Valves | MILITARY | MIL-V-18436 | VALVES, CHECK, BRONZE |
Corrosion Properties