Find suppliers for this alloyC96200
Element | ||||||||||
---|---|---|---|---|---|---|---|---|---|---|
Cu(1) | Pb | Fe | P | Ni(2) | C | Mn | S | Si | Nb(3) | |
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co. (3) When product or casting is intended for subsequent welding applications, and so specified by the purchaser the Nb content shall be 0.40% max. | ||||||||||
Min (%) | 1.0 | 9.0 | ||||||||
Max (%) | Rem | 0.01 | 1.8 | 0.02 | 11.0 | 0.10 | 1.5 | 0.02 | 0.50 | 1.0 |
Form | Temper | Temper Code | Tensile Strength (ksi) | YS-0.5% Ext (ksi) | Elongation (%) | Charpy V-Notch Impact Strength (ft-lbs) | Compressive Strength .1 in. set/in. (ksi) | Fatigue Strength** (ksi) | ||
---|---|---|---|---|---|---|---|---|---|---|
As Sand Cast | As Sand Cast | M01 | 45 Min for Standard 45 Min for Standard 45 Min for Standard | 25 Min for Standard 25 Min for Standard 25 Min for Standard | 20 Min for Standard 20 Min for Standard | 100 Typ | 37 Typ | 13 Typ | ||
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. |
Melting Point - Liquidus°F | 2100 |
---|---|
Melting Point - Solidus°F | 2010 |
Densitylb/cu in. at 68°F | 0.323 |
Specific Gravity | 8.94 |
Electrical Conductivity% IACS at 68°F | 11 |
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 26.1 |
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F) | 9.5 |
Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
Modulus of Elasticity in Tensionksi | 18000 |
Casting Attribute | Level |
---|---|
Casting Yield | Low |
Drossing | Low |
Effect of Section Size | Low |
Fluidity | High |
Gassing | High |
Patternmakers Shrinkageinches per inch | 3/16 |
Shrinkage in Solidification | High |
Technique | Suitability | Footnote |
---|---|---|
Soldering | Excellent | |
Brazing | Excellent | |
Oxyacetylene Welding | Not Recommended | |
Gas Shielded Arc Welding | Poor | Filler metal R CuNi, or E CuNi |
Coated Metal Arc Welding | Fair | Filler metal R CuNi, or E CuNi |
Machinability Rating | 10 |
Common Fabrication Processes
- Casting
Treatment | Value* | Time** | |||
---|---|---|---|---|---|
* Temperature is measured in Fahrenheit. ** Time is measured in minutes. | |||||
Stress Relief | 0 | ||||
Solution Treatment | 0 |
Product Category | Product | Reason Category | Reason |
---|---|---|---|
Industrial | Chemical Processing Equipment | Corrosion Resistance | Corrosion Resistance (Excellent) |
Chemical Processing Equipment | Corrosion Resistance | Erosion and Impingement Resistance | |
Chemical Processing Equipment | Mechanical Properties | High Strength | |
Chemical Processing Equipment | Mechanical Properties | Retains Strength at Elevated Temperatures | |
Components for Oil Refineries | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Components for Oil Refineries | Corrosion Resistance | Erosion and Impingement Resistance | |
Components for Oil Refineries | Mechanical Properties | High Strength | |
Components for Oil Refineries | Mechanical Properties | Retains Strength at Elevated Temperatures | |
Fittings | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Fittings | Mechanical Properties | High Strength | |
Steam Fittings | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Steam Fittings | Corrosion Resistance | Corrosion Resistance to Salt Water | |
Steam Fittings | Mechanical Properties | High Strength | |
Steam Fittings | Mechanical Properties | Retains Strength at Elevated Temperatures | |
Marine | Component Parts for Sea Water Corrosion Resistance. | Corrosion Resistance | Corrosion Resistance (Excellent) |
Component Parts for Sea Water Corrosion Resistance. | Corrosion Resistance | Corrosion Resistance to Salt Water | |
Component Parts for Sea Water Corrosion Resistance. | Corrosion Resistance | Erosion and Impingement Resistance | |
Component Parts for Sea Water Corrosion Resistance. | Mechanical Properties | High Strength | |
Elbows to Resist Sea Water | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Elbows to Resist Sea Water | Corrosion Resistance | Corrosion Resistance to Salt Water | |
Elbows to Resist Sea Water | Mechanical Properties | High Strength | |
Flanges to Resist Sea Water | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Flanges to Resist Sea Water | Corrosion Resistance | Corrosion Resistance to Salt Water | |
Flanges to Resist Sea Water | Mechanical Properties | High Strength | |
Propeller Sleeves to Resist Sea Water | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Propeller Sleeves to Resist Sea Water | Corrosion Resistance | Corrosion Resistance to Salt Water | |
Propeller Sleeves to Resist Sea Water | Corrosion Resistance | Erosion and Impingement Resistance | |
Propeller Sleeves to Resist Sea Water | Mechanical Properties | High Strength | |
Pump Bodies to Resist Sea Water | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Pump Bodies to Resist Sea Water | Corrosion Resistance | Corrosion Resistance to Salt Water | |
Pump Bodies to Resist Sea Water | Mechanical Properties | High Strength | |
Pump Impellers to Resist Sea Water | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Pump Impellers to Resist Sea Water | Corrosion Resistance | Corrosion Resistance to Salt Water | |
Pump Impellers to Resist Sea Water | Corrosion Resistance | Erosion and Impingement Resistance | |
Pump Impellers to Resist Sea Water | Mechanical Properties | High Strength | |
Valves to Resist Sea Water | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Valves to Resist Sea Water | Corrosion Resistance | Corrosion Resistance to Salt Water | |
Valves to Resist Sea Water | Corrosion Resistance | Erosion and Impingement Resistance | |
Valves to Resist Sea Water | Mechanical Properties | High Strength | |
Plumbing | Plumbing Parts | Corrosion Resistance | Corrosion Resistance (Excellent) |
Plumbing Parts | Corrosion Resistance | Erosion and Impingement Resistance | |
Plumbing Parts | Mechanical Properties | High Strength | |
Plumbing Parts | Mechanical Properties | Retains Strength at Elevated Temperatures |
Form | Sub-Form | System | Standard | Description |
---|---|---|---|---|
As Centrifugal Cast | Castings | ASTM | B369 | COPPER NICKEL ALLOY CASTINGS |
Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
Castings | SAE | J462 | CAST COPPER ALLOYS | |
As Sand Cast | Castings | ASTM | B369 | COPPER NICKEL ALLOY CASTINGS |
Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
Castings | SAE | J462 | CAST COPPER ALLOYS | |
Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | |
Valves | MILITARY | MIL-V-18436 | VALVES, CHECK, BRONZE |
Corrosion Properties