Find suppliers for this alloy
C96800
| Elements | ||||||||||
|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | Ni(3) | Mg | Mn | Si | Nb | |
|
(1) The following additional maximum impurity limits shall apply: 0.10% Al, 0.001% B, 0.001% Bi, 0.005% P, 0.0025% S, 0.02% Sb, 0.01%Ti. (2) Cu + Sum of Named Elements 99.5% min. (3) Ni value includes Co. |
||||||||||
| Min (%) | 7.5 | 9.5 | 0.005 | 0.05 | 0.10 | |||||
| Max (%) | Rem | 0.005 | 8.5 | 1.0 | 0.50 | 10.5 | 0.15 | 0.30 | 0.05 | 0.30 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
Elongation (%) |
|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||
| As Sand Cast | As Sand Cast | M01 |
125 Min for Standard |
3 Min for Standard |
| Spinodal Hardened-Low Strength (ATLS) | TX00 |
135 Min for Standard |
||
Physical Properties
Casting Characteristics
Fabrication Properties
Common Fabrication Processes
| Treatment | Minimum* | Value* | Time** | Medium |
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Solution Treatment | 1500 | 2 | Water | |
| Precipitation Treatment | 660 | 5 | ||
Typical Uses
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Sand Cast | Castings | ASTM | B584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | |
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM |
Corrosion Properties