Find suppliers for this alloy
C96970
| Elements | |||||||||
|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | Ni(2) | Mg | Mn | Nb | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co. |
|||||||||
| Min (%) | 5.5 | 8.5 | |||||||
| Max (%) | Rem | 0.02 | 6.5 | 0.50 | 0.50 | 9.5 | 0.15 | 0.30 | 0.10 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Rockwell C scale | Compressive Yield Strength (ksi) |
|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||||
| As Continuous Cast | Spinodal Hardened-Low Strength (ATLS) | TX00 |
105 Min 110 Typ 115 Max |
90 Min 95 Typ 100 Max |
3 Min |
27 Typ |
95 Typ |
| Melting Point - Liquidus°F | 2012 |
|---|---|
| Melting Point - Solidus°F | 1697 |
| Densitylb/cu in. at 68°F | 0.321 |
| Specific Gravity | 8.91 |
| Electrical Conductivity% IACS at 68°F | 13 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 30 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 9 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 9.5 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.7 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.091 |
| Magnetic Permeability | 1.001 |
| Poisson's Ratio | 0.3 |
Casting Characteristics
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Gas Shielded Arc Welding | Excellent |
| Spot Weld | Excellent |
| Seam Weld | Excellent |
| Butt Weld | Excellent |
| Capacity for Being Cold Worked | Good |
| Capacity for Being Hot Formed | Good |
Common Fabrication Processes
- Casting
- Drawing
- Forming and Bending
- Machining
| Treatment | Minimum* | |||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Solution Treatment | 700 | |||
| Annealing | 1400 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Bearings | ||
| Bushings | |||
| Connectors | |||
| Plastic molding tooling | |||
| Retaining Rings | |||
| Valves | |||
| Wear Plates |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Continuous Cast | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS |
Corrosion Properties