Elements | ||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|
Cu(1) | Pb | Sn | Zn | Fe | P | Ni(2) | Al | Mn | S | Sb | Si | |
(1) Cu + Sum of Named Elements 99.7% min. (2) Ni value includes Co. |
||||||||||||
Min (%) | 63.0 | 3.0 | 3.5 | 3.0 | 19.0 | |||||||
Max (%) | 67.0 | 5.0 | 4.5 | 9.0 | 1.5 | 0.05 | 21.5 | 0.005 | 1.0 | 0.08 | 0.25 | 0.15 |
Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load | Charpy V-Notch Impact Strength (ft-lbs) |
Compressive Strength .01 in. set/in. (ksi) |
Compressive Strength .1 in. set/in. (ksi) |
Creep Strength (0.1% per 10,000 hours) (ksi) |
Fatigue Strength** (ksi) |
---|---|---|---|---|---|---|---|---|---|---|---|
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | |||||||||||
As Centrifugal Cast | As Centrifugal Cast | M02 |
40 Min for Standard |
17 Min for Standard |
10 Min for Standard |
||||||
As Continuous Cast | As Continuous Cast | M07 |
40 Min for Standard |
20 Min for Standard |
10 Min for Standard |
||||||
As Sand Cast | As Sand Cast | M01 |
40 Min for Standard 45 Typ |
17 Min for Standard 24 Typ |
10 Min for Standard 20 Typ |
80 Typ |
11 Typ |
30 Typ | 57 Typ | 33 Typ | 16 Typ |
Melting Point - Liquidus°F | 2089 |
---|---|
Melting Point - Solidus°F | 2027 |
Densitylb/cu in. at 68°F | 0.321 |
Specific Gravity | 8.9 |
Electrical Conductivity% IACS at 68°F | 5 |
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 13 |
Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.3 |
Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
Modulus of Elasticity in Tensionksi | 19000 |
Casting Attribute | Level |
---|---|
Casting Yield | Medium |
Drossing | Med-High |
Effect of Section Size | Medium |
Fluidity | High |
Gassing | Med-High |
Patternmakers Shrinkage inches per inch | 2/16 |
Shrinkage in Solidification | Medium |
Technique | Suitability |
---|---|
Soldering | Excellent |
Brazing | Excellent |
Oxyacetylene Welding | Not Recommended |
Gas Shielded Arc Welding | Not Recommended |
Coated Metal Arc Welding | Not Recommended |
Machinability Rating | 70 |
Common Fabrication Processes
Treatment | Value* | Time** | ||
---|---|---|---|---|
* Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
Stress Relief | 500 | |||
Solution Treatment | 0 |
Product Category | Product | Reason Category | Reason |
---|---|---|---|
Architecture | Ornamental Castings | Appearance | Pleasing Silver Color |
Ornamental Castings | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Ornamental Castings | Machining Properties | Machinability, Good | |
Ornamental Castings | Mechanical Properties | Moderate Strength | |
Builders Hardware | Door Hardware for Prison Doors | Appearance | Pleasing Silver Color |
Door Hardware for Prison Doors | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Door Hardware for Prison Doors | Machining Properties | Machinability, Good | |
Door Hardware for Prison Doors | Mechanical Properties | Moderate Strength | |
Hardware | Appearance | Pleasing Silver Color | |
Hardware | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Hardware | Machining Properties | Machinability, Good | |
Hardware | Mechanical Properties | Moderate Strength | |
Window Hardware | Appearance | Appearance | |
Window Hardware | Appearance | Pleasing Silver Color | |
Window Hardware | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Window Hardware | Machining Properties | Machinability, Good | |
Window Hardware | Mechanical Properties | Moderate Strength | |
Consumer | Piano Keys | Appearance | Pleasing Silver Color |
Piano Keys | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Piano Keys | Machining Properties | Machinability, Good | |
Piano Keys | Mechanical Properties | Moderate Strength | |
Industrial | Pumps | Corrosion Resistance | Corrosion Resistance (Excellent) |
Pumps | Machining Properties | Machinability, Good | |
Pumps | Mechanical Properties | Moderate Strength | |
Valves | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Valves | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Valves | Machining Properties | Machinability, Good | |
Valves | Mechanical Properties | Moderate Strength | |
Marine | Marine Furniture | Appearance | Pleasing Silver Color |
Marine Furniture | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Marine Furniture | Machining Properties | Machinability, Good | |
Marine Furniture | Mechanical Properties | Moderate Strength | |
Plumbing | Sanitary Fittings | Corrosion Resistance | Corrosion Resistance |
Sanitary Fittings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Sanitary Fittings | Machining Properties | Machinability, Good | |
Sanitary Fittings | Mechanical Properties | Moderate Strength |
Form | Specific Sub-Form | Application | System | Standard | Description |
---|---|---|---|---|---|
As Centrifugal Cast | Castings | ASTM | B271/B271M | COPPER BASE ALLOY CENTRIFUGAL CASTINGS | |
As Continuous Cast | Castings | SAE | J462 | CAST COPPER ALLOYS | |
Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
Castings | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | ||
As Sand Cast | Castings | ASTM | B763/B763M | COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS | |
Castings | ASME | SB584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | ||
Castings | ASTM | B584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | ||
Ingot | |||||
ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | |||
Valves | MILITARY | MIL-V-18436 | VALVES, CHECK, BRONZE |
Corrosion Properties