Find suppliers for this alloy
C97800
| Elements | ||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P | Ni(2) | Al | Mn | S | Sb | Si | |
|
(1) Cu + Sum of Named Elements 99.6% min. (2) Ni value includes Co. |
||||||||||||
| Min (%) | 64.0 | 1.0 | 4.0 | 1.0 | 24.0 | |||||||
| Max (%) | 67.0 | 2.5 | 5.5 | 4.0 | 1.5 | 0.05 | 27.0 | 0.005 | 1.0 | 0.08 | 0.20 | 0.15 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 3000 kg load |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| As Centrifugal Cast | As Centrifugal Cast | M02 |
50 Min for Standard |
22 Min for Standard |
10 Min for Standard |
|
| As Continuous Cast | As Continuous Cast | M07 |
45 Min for Standard |
22 Min for Standard |
8 Min for Standard |
|
| As Sand Cast | As Sand Cast | M01 |
50 Min for Standard 55 Typ |
22 Min for Standard 30 Typ |
10 Min for Standard 15 Typ |
130 Typ |
| Melting Point - Liquidus°F | 2156 |
|---|---|
| Melting Point - Solidus°F | 2084 |
| Densitylb/cu in. at 68°F | 0.32 |
| Specific Gravity | 8.86 |
| Electrical Conductivity% IACS at 68°F | 4 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 14.7 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.7 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 19000 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | Medium |
| Drossing | Med-High |
| Effect of Section Size | Medium |
| Fluidity | High |
| Gassing | Med-High |
| Patternmakers Shrinkage inches per inch | 3/16 |
| Shrinkage in Solidification | Medium |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Machinability Rating | 60 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 500 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Architecture | Ornamental Castings | Appearance | Pleasing Silver Color |
| Ornamental Castings | Corrosion Resistance | Corrosion Resistance | |
| Ornamental Castings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Ornamental Castings | Mechanical Properties | Moderate Strength | |
| Builders Hardware | Hardware | Appearance | Appearance |
| Hardware | Appearance | Pleasing White Color | |
| Hardware | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Hardware | Mechanical Properties | Moderate Strength | |
| Consumer | Musical Instruments Components | Appearance | Pleasing Silver Color |
| Musical Instruments Components | Corrosion Resistance | Corrosion Resistance | |
| Musical Instruments Components | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Musical Instruments Components | Mechanical Properties | Moderate Strength | |
| Industrial | Fittings for Diary and Food Processing | Appearance | Pleasing White Color |
| Fittings for Diary and Food Processing | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Fittings for Diary and Food Processing | Corrosion Resistance | Corrosion Resistance to Milk | |
| Fittings for Diary and Food Processing | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Fittings for Diary and Food Processing | Mechanical Properties | Moderate Strength | |
| Valves | Corrosion Resistance | Corrosion Resistance | |
| Valves | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Valves | Mechanical Properties | Moderate Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Centrifugal Cast | Castings | ASTM | B271/B271M | COPPER BASE ALLOY CENTRIFUGAL CASTINGS | |
| As Continuous Cast | Castings | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | |
| As Sand Cast | Castings | ASTM | B763/B763M | COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS | |
| Castings | ASTM | B584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | ||
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | ||
| Valves | MILITARY | MIL-V-18436 | VALVES, CHECK, BRONZE |
Corrosion Properties