Find suppliers for this alloy
C99300
| Elements | ||||||||
|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Fe | Ni | Al | Co | Si | |
|
(1) Cu + Sum of Named Elements 99.7% min. |
||||||||
| Min (%) | 0.40 | 13.5 | 10.7 | 1.0 | ||||
| Max (%) | Rem | 0.02 | 0.05 | 1.0 | 16.5 | 11.5 | 2.0 | 0.02 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 3000 kg load | Charpy V-Notch Impact Strength (ft-lbs) |
Proportional Limit (ksi) |
|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||||
| As Sand Cast | As Sand Cast | M01 |
95 Typ |
55 Typ |
2 Typ |
200 Typ |
4 Typ |
28 Typ |
| Melting Point - Liquidus°F | 1970 |
|---|---|
| Melting Point - Solidus°F | 1955 |
| Densitylb/cu in. at 68°F | 0.275 |
| Specific Gravity | 7.61 |
| Electrical Conductivity% IACS at 68°F | 9 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 25 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.2 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.1 |
| Modulus of Elasticity in Tensionksi | 18000 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | Low |
| Drossing | High |
| Effect of Section Size | Low |
| Fluidity | Medium |
| Gassing | Medium |
| Patternmakers Shrinkage inches per inch | 3/16 |
| Shrinkage in Solidification | High |
| Technique | Suitability |
|---|---|
| Soldering | Not Recommended |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Good |
| Machinability Rating | 20 |
Common Fabrication Processes
| Treatment | Value* | Time** | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 950 | |||
| Solution Treatment | 0 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Corrosion and Scaling Resistant Parts | Appearance | Pleasing White Color |
| Corrosion and Scaling Resistant Parts | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Corrosion and Scaling Resistant Parts | Corrosion Resistance | Oxidation Resistance | |
| Corrosion and Scaling Resistant Parts | Mechanical Properties | Moderate Strength | |
| Corrosion and Scaling Resistant Parts | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Glass Making Molds | Conductivity (Thermal) | Thermal Conductivity | |
| Glass Making Molds | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Glass Making Molds | Mechanical Properties | Moderate Strength | |
| Glass Making Molds | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Parts Requiring High Thermal Conductivity | Conductivity (Thermal) | Thermal Conductivity | |
| Parts Requiring High Thermal Conductivity | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Parts Requiring High Thermal Conductivity | Corrosion Resistance | Oxidation Resistance | |
| Parts Requiring High Thermal Conductivity | Mechanical Properties | Moderate Strength | |
| Parts Requiring High Thermal Conductivity | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Rolls for Making Plate Glass | Conductivity (Thermal) | Thermal Conductivity | |
| Rolls for Making Plate Glass | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Rolls for Making Plate Glass | Mechanical Properties | Moderate Strength | |
| Rolls for Making Plate Glass | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Marine | Marine Hardware | Appearance | Appearance |
| Marine Hardware | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Marine Hardware | Mechanical Properties | Moderate Strength |
Applicable Specifications
Corrosion Properties