Find suppliers for this alloy
C99500
| Elements | ||||||||
|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Zn | Fe | Ni | Al | Mn | Si | |
|
(1) Cu + Sum of Named Elements 99.7% min. |
||||||||
| Min (%) | 0.50 | 3.0 | 3.5 | 0.50 | 0.50 | |||
| Max (%) | Rem | 0.09 | 2.0 | 5.0 | 5.50 | 2.0 | 0.50 | 2.0 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load | Brinell Hardness, 3000 kg load | Proportional Limit (ksi) |
|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||||
| As Sand Cast | As Sand Cast | M01 |
70 Min for Standard |
40 Min for Standard |
12 Min for Standard |
145 Typ |
50 Typ |
21 Typ |
| Precipitation Hardened | TF00 |
86 Typ |
62 Typ |
8 Typ |
196 Typ |
|||
| Densitylb/cu in. at 68°F | 0.3 |
|---|---|
| Specific Gravity | 8.3 |
| Electrical Conductivity% IACS at 68°F | 10 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 8.3 |
| Modulus of Elasticity in Tensionksi | 19000 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | Low |
| Drossing | Medium |
| Effect of Section Size | Low |
| Fluidity | Medium |
| Gassing | Low |
| Patternmakers Shrinkage inches per inch | 3/16 |
| Shrinkage in Solidification | High |
| Technique | Suitability |
|---|---|
| Gas Shielded Arc Welding | Good |
| Machinability Rating | 50 |
Common Fabrication Processes
| Treatment | Minimum* | Value* | Time** | Medium |
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 600 | |||
| Solution Treatment | 1625 | 60 | Water | |
| Precipitation Treatment | 900 | 60 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Electrical | Electrical Parts | Conductivity (Electrical) | Electrical Conductivity |
| Electrical Parts | Conductivity (Thermal) | Thermal Conductivity | |
| Electrical Parts | Corrosion Resistance | Corrosion Resistance | |
| Electrical Parts | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Electrical Parts | Mechanical Properties | Moderate Strength | |
| Electrical Parts | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Industrial | Gears for Mining Equipment | Corrosion Resistance | Corrosion Resistance |
| Gears for Mining Equipment | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Gears for Mining Equipment | Mechanical Properties | Moderate Strength | |
| Gears for Mining Equipment | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Propeller Wheels | Corrosion Resistance | Corrosion Resistance | |
| Propeller Wheels | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Propeller Wheels | Mechanical Properties | Moderate Strength | |
| Propeller Wheels | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Valve Stems | Corrosion Resistance | Corrosion Resistance | |
| Valve Stems | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Valve Stems | Mechanical Properties | Moderate Strength | |
| Valve Stems | Mechanical Properties | Retains Strength at Elevated Temperatures | |
| Marine | Outboard Marine Components | Corrosion Resistance | Corrosion Resistance |
| Outboard Marine Components | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Outboard Marine Components | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Outboard Marine Components | Mechanical Properties | Moderate Strength | |
| Outboard Marine Components | Mechanical Properties | Retains Strength at Elevated Temperatures |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Continuous Cast | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | ||
| As Sand Cast | Castings | ASTM | B763/B763M | COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS | |
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM |
Corrosion Properties