Find suppliers for this alloy
C99700
| Elements | ||||||||
|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | Ni | Al | Mn | |
|
(1) Cu + Sum of Named Elements 99.7% min. |
||||||||
| Min (%) | 54.0 | 19.0 | 4.0 | 0.50 | 11.0 | |||
| Max (%) | 2.0 | 1.0 | 25.0 | 1.0 | 6.0 | 3.0 | 15.0 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 3000 kg load |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| As Die Cast | As Pressure Die Cast | M04 |
65 Typ |
27 Typ |
15 Typ |
125 Typ |
| As Sand Cast | As Sand Cast | M01 |
55 Typ |
25 Typ |
25 Typ |
110 Typ |
| Melting Point - Liquidus°F | 1655 |
|---|---|
| Melting Point - Solidus°F | 1615 |
| Densitylb/cu in. at 68°F | 0.296 |
| Specific Gravity | 8.19 |
| Electrical Conductivity% IACS at 68°F | 3 |
| Modulus of Elasticity in Tensionksi | 16500 |
| Casting Attribute | Level |
|---|---|
| Casting Yield | Medium |
| Drossing | Medium |
| Effect of Section Size | Low |
| Fluidity | High |
| Gassing | Low |
| Patternmakers Shrinkage inches per inch | 4/16 |
| Shrinkage in Solidification | Medium |
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Good |
| Oxyacetylene Welding | Good |
| Machinability Rating | 80 |
Common Fabrication Processes
| Treatment | Minimum* | Value* | Time** | |
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
| Stress Relief | 700 | |||
| Solution Treatment | 0 | |||
| Precipitation Treatment | 932 | |||
| Annealing | 842 | |||
Typical Uses
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| As Die Cast | Castings | ASTM | B176 | BRASS DIE CASTINGS | |
| Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM |
Corrosion Properties