Find suppliers for this alloyC22600
Chemical Composition
Element
Cu(1)PbZnFe
(1) Cu + Sum of Named Elements 99.8% min.
Min (%)86.0
Max (%)89.00.05Rem0.05
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Shear Strength
(ksi)
Torsion Modulus
(ksi)
Ultimate Tensile Strength in Shear
(ksi)
Section Size
(in)
Flat Products1/2 HardH0254   Typ
47   Typ
12   Typ
61   Typ
36   Typ
0.04
1/4 HardH0147   Typ
37   Typ
25   Typ
47   Typ
34   Typ
0.04
Extra HardH0672   Typ
60   Typ
4   Typ
78   Typ
42   Typ
0.04
HardH0466   Typ
56   Typ
5   Typ
73   Typ
40   Typ
0.04
Nominal Grain Size 0.015 mmOS01544   Typ
16   Typ
42   Typ
68   Typ
32   Typ
0.04
Nominal Grain Size 0.025 mmOS02542   Typ
15   Typ
44   Typ
64   Typ
31   Typ
0.04
Nominal Grain Size 0.035 mmOS03540   Typ
13   Typ
45   Typ
59   Typ
30   Typ
0.04
Nominal Grain Size 0.050 mmOS05039   Typ
11   Typ
46   Typ
55   Typ
29   Typ
0.04
SpringH0879   Typ
62   Typ
4   Typ
82   Typ
44   Typ
6.4   Typ
0.04
Flat Products & Wire1/2 HardH0254   Typ
47   Typ
12   Typ
36   Typ
0.04
H0268   Typ
60   Typ
7   Typ
40   Typ
0.08
Nominal Grain Size 0.015 mmOS01544   Typ
16   Typ
42   Typ
32   Typ
0.04
OS01545   Typ
18   Typ
38   Typ
32   Typ
0.08
Nominal Grain Size 0.050 mmOS05039   Typ
11   Typ
46   Typ
29   Typ
0.04
OS05040   Typ
13   Typ
44   Typ
29   Typ
0.08
SpringH0879   Typ
62   Typ
4   Typ
44   Typ
0.04
H0897   Typ
66   Typ
3   Typ
0.08
Wire1/2 HardH0268   Typ
7   Typ
70   Typ
40   Typ
0.08
1/4 HardH0156   Typ
12   Typ
36   Typ
0.08
1/8 HardH0047   Typ
26   Typ
34   Typ
0.08
Extra HardH0689   Typ
4   Typ
0.08
HardH0483   Typ
5   Typ
0.08
Nominal Grain Size 0.015 mmOS01545   Typ
18   Typ
38   Typ
32   Typ
0.08
Nominal Grain Size 0.025 mmOS02543   Typ
40   Typ
31   Typ
0.08
Nominal Grain Size 0.035 mmOS03541   Typ
18   Typ
42   Typ
30   Typ
0.08
Nominal Grain Size 0.050 mmOS05040   Typ
44   Typ
29   Typ
0.08
SpringH0897   Typ
3   Typ
0.08
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1895
Melting Point - Solidus°F1840
Densitylb/cu in. at 68°F0.317
Specific Gravity8.78
Electrical Conductivity% IACS at 68°F40
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F100
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)10.3
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi17000
Modulus of Rigidityksi6400
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingNot Recommended
Spot WeldFair
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedGood
Machinability Rating30
Common Fabrication Processes
  • Blanking
  • Coining
  • Drawing
  • Etching
  • Forming and Bending
  • Heading and Upsetting
  • Piercing and Punching
  • Roll Threading and Knurling
  • Shearing
  • Spinning
  • Squeezing and Swaging
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8001400
Hot Treatment14001650
Typical uses
Product Category Product Reason Category Reason
ArchitectureAnglesAppearanceAppearance
AnglesAppearanceColor
AnglesCorrosion ResistanceCorrosion Resistance
AnglesForming CharacteristicsFormability
AnglesMechanical PropertiesModerate Strength
ChannelsAppearanceAppearance
ChannelsCorrosion ResistanceCorrosion Resistance
ChannelsForming CharacteristicsFormability
ChannelsMechanical PropertiesModerate Strength
ConsumerChain LinksAppearanceAppearance
Chain LinksCorrosion ResistanceCorrosion Resistance
Chain LinksCorrosion ResistanceCorrosion Resistance to Fresh Water
Chain LinksCorrosion ResistanceCorrosion Resistance to Salt Water
Chain LinksForming CharacteristicsFormability
Chain LinksMechanical PropertiesHigh Strength
CompactsAppearanceAppearance
CompactsAppearanceColor
CompactsCorrosion ResistanceCorrosion Resistance
CompactsForming CharacteristicsFormability
CompactsMechanical PropertiesModerate Strength
Costume JewelryAppearanceAppearance
Costume JewelryForming CharacteristicsFormability
Costume JewelryPlating CharacteristicsBase for Gold Plate
EmblemsAppearanceAppearance
EmblemsAppearanceColor
EmblemsCorrosion ResistanceCorrosion Resistance
EmblemsForming CharacteristicsFormability
EmblemsMechanical PropertiesModerate Strength
Etched ArticlesAppearanceAppearance
Etched ArticlesAppearanceColor
Etched ArticlesCorrosion ResistanceCorrosion Resistance
Etched ArticlesForming CharacteristicsFormability
Etched ArticlesMechanical PropertiesModerate Strength
Lipstick ContainersAppearanceAppearance
Lipstick ContainersAppearanceColor
Lipstick ContainersCorrosion ResistanceCorrosion Resistance
Lipstick ContainersForming CharacteristicsFormability
Lipstick ContainersMechanical PropertiesModerate Strength
PlaquesAppearanceAppearance
PlaquesAppearanceColor
PlaquesCorrosion ResistanceCorrosion Resistance
PlaquesForming CharacteristicsFormability
PlaquesMechanical PropertiesModerate Strength
ZippersAppearanceColor
ZippersCorrosion ResistanceCorrosion Resistance
ZippersForming CharacteristicsCold Workability
ElectricalRotor Bars, AC MotorsBrazing CharacteristicsBrazability
Rotor Bars, AC MotorsConductivity (Electrical)Electrical Resistivity - 40 % IACS
FastenersEyeletsAppearanceAppearance
EyeletsCorrosion ResistanceCorrosion Resistance
EyeletsForming CharacteristicsFormability
EyeletsMechanical PropertiesModerate Strength
FastenersAppearanceAppearance
FastenersCorrosion ResistanceCorrosion Resistance
FastenersMechanical PropertiesModerate Strength
Slide FastenersCorrosion ResistanceCorrosion Resistance
Slide FastenersForming CharacteristicsFormability
Slide FastenersMechanical PropertiesModerate Strength
Applicable Specifications
Form System Standard Description
BarASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
PlateASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
SheetASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
StripASTMB36/B36MBRASS PLATE, SHEET, STRIP AND ROLLED BAR
WireASTMB134/B134MBRASS WIRE
Corrosion Properties

No information available.